Postby Sancho's Horse » Fri Jun 29, 2012 1:31 pm

I have some stainless steel bar stock that I was going to use as a spacer on an aluminum trailer I am building. I am a little worried about galvanic effects. Should I be? I was considering using some JB weld to provide some added strength and was hoping that this might slow these effects.

Does anyone have any best practice experience?

I had someone tell me because it is stainless it will be fine, but they based this on nothing. I try to know enough to know when I don't know.
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Harold in CR » Fri Jun 29, 2012 2:03 pm

From past experience in manufacturing using SS, we always used NON-magnetic 304 Stainless. Outboard motors are used in a very corrosive environment. SS bolts and screws are used, BUT, the corrosive environment will cause the Aluminum to corrode and stick to the SS.

I'm sure there are others with better metallurgy info, and, we were told 304 is NOT non-magnetic and WILL rust or corrode, but, we never had to replace anything we built due to what we used, mostly the product was used in Salt Water.. When in doubt, a tiny dab of a non-stick compound, like "Never Seize" will stop the "Galvanic action" by keeping the corrosive aluminum from sticking to the NON corrosive SS.

18 years of doing the SS stuff, is what I am offering as advice.
Thanks to Justin, the forum is open source and NON-commercialized.

http://www.costaricacraftwood.com
Harold in CR
100 kW
100 kW
 
Posts: 1115
Joined: Mon Feb 01, 2010 7:19 pm
Location: Costa Rica

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby marty » Fri Jun 29, 2012 4:20 pm

ebikes.ca
Online resource for electric bicycle conversions

http://www.ebikes.ca
Image
MARTY
Volt Electric Vehicles
http://www.voltev.com
User avatar
marty
100 kW
100 kW
 
Posts: 1155
Joined: Thu Apr 19, 2007 5:44 pm
Location: Buffalo, New York USA

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby iamsofunny » Fri Jun 29, 2012 11:14 pm

The aluminum will corrode in the slightest from the galvanic effect, not the stainless
The stainless will rust by itself eventually
iamsofunny
100 W
100 W
 
Posts: 142
Joined: Mon Apr 30, 2012 8:43 pm

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Tench » Sat Jun 30, 2012 4:22 am

The link below is to a Galvanic list, basically the most reactive metals are near the top and least at the bottom, a basic rule is the greater the distance on the list between 2 adjoining metals, the greater the Galvanic reaction. Select materials that are closer together to minimise reaction.

http://www.eaa1000.av.org/technicl/corr ... lvanic.htm
Project Two viewtopic.php?f=6&t=37489
Project one viewtopic.php?f=28&t=20304&hilit=tench

The uk's first Stealth Bomber
Tench
1 kW
1 kW
 
Posts: 423
Joined: Tue Jul 13, 2010 12:48 pm
Location: UK

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Kingfish » Sat Jun 30, 2012 3:30 pm

I bet if you offered up a sacrificial anode that it will reduce the potential:
Imagine the in-line short check-valve to a water heater, or the replaceable anode rods: The anode takes the brunt of the ionic potential before considering the tasty insides of the water heater and the heating elements… in theory anyway. On Navy ships where steam is employed, the main condenser turns spent steam back into feedwater, and does this by passing seawater through cooling tubes: On the seawater side there are large plates of Cadmium (or Zinc alloy) that act as the sacrificial anode, and these had to be inspected/replaced periodically.

First see if you can get Cadmium washers, and second - place a few on the trailer in easily observed areas… and that should take care of the potential. :)

Passivated, KF
* My 2WD Garden Wall
* Current ride: 2WD Disc EBikeKit (9C 2806-equivalent) / Dual Lyen 12FET / 15S6P LiPo when commuting.
* Going to California: 2011: Trip completed 8)
* Club Member: 40-mph & 101. 10k-Club: 9634 miles-to-date, 4144 as 2WD.

It is by caffeine alone I set my mind in motion.
It is by the beans of Java that thoughts acquire speed.
The hands acquire shakes, the shakes become a warning.
It is by caffeine alone I set my mind in motion.
User avatar
Kingfish
1.21 GW
1.21 GW
 
Posts: 3504
Joined: Wed Feb 03, 2010 11:23 am
Location: Redmond, WA-USA, Earth, Sol, Orion–Cygnus Arm, Milky Way. Age: > yesterday < tomorrow

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby iamsofunny » Sat Jun 30, 2012 3:46 pm

The glue would help if it's waterproof
iamsofunny
100 W
100 W
 
Posts: 142
Joined: Mon Apr 30, 2012 8:43 pm

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Sancho's Horse » Sat Jun 30, 2012 11:00 pm

Thanks for the responses. The Stainless in question is 316 stainless strip bar (non-magnetic). Tench put up a really useful list from an Army Missile Command Report RS-TR-67-11, thanks for that. I think the Aluminum in question is 6061 T6, but that is just a guess. It is some extruded support for a dry erase board. I have cut it before, many months ago, and had parts in corrosive environments, and didn't notice any big difference in corrosion between the outside and the cut portions, however, there is some sort of coating.

I checked out the JB Weld. They say water-proof, electrically insulating, acid resistant, and good enough for me. There is probably something better suited out there, but I am familiar with it, and it is cheap so, I will end up using it. Above and beyond the usual sanding and cleaning of surfaces, I will put some deep scratches in the aluminum before I apply any of the JB Weld.

Originally, I was going to use some of the 1/4" Aluminum bits from the base of the dry erase board to strengthen the joint, but another idea came along which required those pieces. Of course, inspiration struck only a day or two after I had already made the cuts, so now we have spacers, and I am on my usual path to knowledge. Most of the useful bits usually come after I say, "Oh, no!"
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby iamsofunny » Sat Jun 30, 2012 11:31 pm

Don't use the glue as your only method of adhesion. It's more of a protective layer.
If something is slightly wrong and an aluminum oxide layer forms (that's the stuff you saw on the aluminum) the glue will just come right off
Aluminum doesn't glue well anyway
iamsofunny
100 W
100 W
 
Posts: 142
Joined: Mon Apr 30, 2012 8:43 pm

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Sancho's Horse » Sat Jun 30, 2012 11:46 pm

Good point. I am using some stainless steel screws to attach to one piece, and SS carriage bolts for the other portion. I have some large HDPE chunks I may stick in one tube to reduce some of the sheer stress on the screws.

Can you tell I reflexively overbuild? But, my stuff lasts...until it doesn't.
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Jeremy Harris » Sun Jul 01, 2012 5:27 am

The best stuff for preventing galvanic corrosion is the stuff specifically made for the purpose and used worldwide on ships and aircraft, zinc chromate paste (also known colloquially as "gorilla snot" by those who use it a lot - once you see it you'll realise why.........). It's readily available in tubes or tins and does an excellent job with alloy and ferrous metal bolted/riveted joints. These are the people I've bought the stuff from over the years: http://www.lasaero.com/site/products/ar ... =P002OHHP1 but a web search for "zinc chromate paste" should find people in your part of the world that sell it, usually under the Duralac, JC5A or Polycast brand names.
Please ask questions on the forum, rather than by PM, as it helps others and you'll get a better range of answers.
User avatar
Jeremy Harris
10 GW
10 GW
 
Posts: 4635
Joined: Tue Oct 23, 2007 4:15 pm
Location: Salisbury, UK

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Sancho's Horse » Sun Jul 01, 2012 9:29 pm

If I can use something called gorilla snot, and its use is likely best practice, this is among the most compelling arguments in my life. Thanks, Jeremy. I will check it out.
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby TylerDurden » Sun Jul 01, 2012 9:44 pm

Sancho's Horse wrote:If I can use something called gorilla snot, and its use is likely best practice, this is among the most compelling arguments in my life.
:lol:

Around here, we use Permatex Anti-Seize for steel bolts into aluminum cylinder heads. I also dollop the stuff onto alloy wheels to keep them from bonding to steel hubs.
Have a Nice Day,

TD

Image
___________________________________________________________

FYI: Adding pictures?

Bored?... take a crack at the unanswered posts

Please post your Watts-at-speed in the survey.



Image
User avatar
TylerDurden
100 GW
100 GW
 
Posts: 8540
Joined: Thu Jan 04, 2007 5:50 pm
Location: Wear the fox hat.

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Chalo » Mon Jul 02, 2012 12:17 am

Sancho's Horse wrote:I have some stainless steel bar stock that I was going to use as a spacer on an aluminum trailer I am building. I am a little worried about galvanic effects. Should I be? I was considering using some JB weld to provide some added strength and was hoping that this might slow these effects.

Does anyone have any best practice experience?

I had someone tell me because it is stainless it will be fine, but they based this on nothing. I try to know enough to know when I don't know.


Stainless fasteners in aluminum parts are utterly ubiquitous. If you are worried about it, add some grease to the contact surfaces before assembling. There are probably ten other things that will kill your gizmo before any kind of corrosion does. Why do you want to make this more complicated than it is?

Chalo
This is to express my gratitude to Justin of Grin Technologies for his extraordinary measures to save this forum for the benefit of all.
User avatar
Chalo
1 MW
1 MW
 
Posts: 1884
Joined: Wed Apr 29, 2009 11:29 pm
Location: Austin, Texas

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Sancho's Horse » Mon Jul 02, 2012 9:10 pm

There are experts and some well reasoned thinkers on this forum. If I have a pretty good idea about a wheel question (or whatever), I am still going to research/ask it, because other people know more than I do on many subjects. Even if I think I am an expert, I am often surprised by what I learn by asking.

Hard to argue with results. Look at the information posted. Good stuff.

How did you know my contraption has been designed to fall apart?
I consider it the trailer equivalent of give a penny take a penny.
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Chalo » Mon Jul 02, 2012 9:14 pm

Sancho's Horse wrote:How did you know my contraption has been designed to fall apart?
I consider it the trailer equivalent of give a penny take a penny.


I said no such thing; I only meant that galvanic corrosion should be somewhere near the bottom of your list of worries. Outside of some problems with carbon fiber and titanium bike parts, I have never known it to be a significant issue with bikes.

Chalo
This is to express my gratitude to Justin of Grin Technologies for his extraordinary measures to save this forum for the benefit of all.
User avatar
Chalo
1 MW
1 MW
 
Posts: 1884
Joined: Wed Apr 29, 2009 11:29 pm
Location: Austin, Texas

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Sancho's Horse » Mon Jul 02, 2012 9:34 pm

Only kidding. You are right about this corrosion for structural integrity, but it is in a very visible spot on a trailer I want people to look at. So, it was purely a cosmetic consideration.

The knowledge gained is structural.
Sancho's Horse
1 kW
1 kW
 
Posts: 377
Joined: Tue Aug 09, 2011 2:27 pm
Location: Muncie, Indiana (USA) or Beijing or Tianjin (China)

Re: Galvanic Effects Stainless Steel vs. Aluminum

Postby Jeremy Harris » Tue Jul 03, 2012 3:50 am

I've made several trailers out of aluminium alloy rectangular/square tube and stainless bolts/rivets over the years. All have lived outside, some, like the boat trailer pictured below, have been in seawater a few times. None have ever shown any significant corrosion, apart for the normal thin layer of oxide aluminium alloy gets after being outside for a while. All the bolts and rivets get smeared with Duralac zinc chromate paste before being fitted, which 100% prevents any galvanic corrosion. The trailer photo below was taken after a couple of years use and exposure.

Trailer 3.JPG
Please ask questions on the forum, rather than by PM, as it helps others and you'll get a better range of answers.
User avatar
Jeremy Harris
10 GW
10 GW
 
Posts: 4635
Joined: Tue Oct 23, 2007 4:15 pm
Location: Salisbury, UK


Return to General Discussion

Who is online

Users browsing this forum: No registered users and 4 guests