Post by rojitor » Jun 23, 2017 6:01 am

I just got a couple days ago a custom spot welder. It has tons of potential so i want to share this info with the community.
I live in a small house, we are swimming on electric and painting stuff so i can't afford to have big machines. I looked for small custom spot welders on the net: microwave, car battery, supercapacitors.... all of them too big or not what i was aiming for. Then i found this welder. It's not a new device, was created time ago, since it is interesting many guys tried to buy it and the creator sold a few in his area but refused for a long time to ship overseas, i guess it's looong time consuming for a low profit.
People insisted so recently he opened his hands to the world and i managed to get one for me. I'll make a small review.

Image
It's made out of arduino custom shields. The creator is a korean genius named Aulakiria. He did many prototypes, ac powered...dremel size...this is the final item.
It's powered by a 3s lipo, YES! lipo hates being shorted but he managed to limit the short to 16ms so no damage at all. The size is minimal 4x3x8 cm.
Image
This is how i got it. The module, a pen, a momentary switch for manual use and a hakko solder iron (It solders as well) The shipping was incredibly fast 7 days from korea.
Image
He sent me as a courtesy some nickel strips and the matching xt90 connector for the lipo.
Image
everything fits inside this small box. PERFECT! my dream size.
All you need is a 3s lipo to use it. Just solder the xt90 and you are done. Aulakiria recommends top lipos, above 40c. It will work with whatever you have but the better the lipo the better the welds. He even did the demos with crappy b grade 25c to prove it.
Image
It has top quality IFR1404 mosfet manufactured in Korea and Taiwan. He recommends to keep the mosfet under 50º celsius. The shield has a port for a 5v fan. The left side is negative and the right side is positive.
Image
I installed a fan but totally failed. The temperature was always high, the welder stops automatically to avoid damage.
So annoying! My country is VERY HOT these days.
Image

Well...maybe not that hot but very hot anyway so i installed some heat sinks on the plate.
Image
Image
and two 12 volt fans.The temperature never goes above 30º celsius now.
Image
In normal conditions any 5v will do a perfect performance. If you have a soft weather there's no need to mod.
mod video:


I did a small video to show the performance:

To use the hakko solder you need a power supply 12-35v. 19+ prefered .Any laptop power supply will do.
Image
This is me testing the iron

This is Aulakiria himself using the iron:

Aulakiria translated the menu so we can read it. It's easy to play.
Image
using it:


in depth testing


The welding times are usually:
For nickel strips
0.1 1.4ms
0.15 4ms
0.20 7ms
The machine is copper welding capable but requires 4s lipo. That is dangerous for the machine and yourself. The intense use of 4s lipo on high flux times may cause premature failure of the machine. Use it at your own risk.
copper times are:
0.1 5-6 ms x2
0.2 10-12 ms x4
Do not use copper unless you know what you are doing. The use of gloves and glasses are mandatory.

when the A is blinking is ready to weld in the waiting time you set. When manual set selected it will weld when you press the button. I plan to install a pedal.
My honest verdict:
if you are low on budget,have a small house and you just make small packs every now and then like me this is perfect.
If you have a huge garage plenty of room, you can afford semi-professional machines and/or you do intensive use of spot welder maybe you prefer something bigga hardda fastta strongga.

DISCLAIMER:
I am not affiliated, associated, authorized, endorsed by, or in any way officially connected with Aulakiria. THIS IS NOT A SALES THREAD. And i have no profit nor gain with this, i just think it's a nice thing and i am sharing it with you. If you are interested on buying one just mail him saying you want one here aulakiria@naver.com that's his paypal account as well. If you mail him be brief and use only perfect academic understandable english. Something google translator can deal with.
The prices are :
basic set : usd $ 80
Hakko T12 soldering iron Handle & Tip : usd $15 (option)
full set : usd $95
Paypal fees 3.5%, Usd-krw Exchange fees 3%...It is double charged so please consider the option send money to family/friend
shipping method
1. Global RR (KOREA post registered airmail) : $15 (20~40 business days)
2. Global EMS fee : $25 (10~15 business days)
more info here: https://m.blog.naver.com/aulakiria/220992039512
Last edited by rojitor on Sep 11, 2017 6:21 pm, edited 13 times in total.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 23, 2017 6:02 am

Aulakiria automatic spot welding

testing


dremel size prototype


PORN TIME

Image
Image
dremel size

Image
arduino custom shields

Image
IFR1404 mosfet installation
Image
Image
version 0.9 ready

Image
0.9 vs 1.0 (solder added)
Last edited by rojitor on Jun 24, 2017 5:46 am, edited 1 time in total.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

BATTERY BUILDS

Post by rojitor » Jun 23, 2017 6:09 am

6S1P Li-ion 18650 LG mg1 with pure copper 0.1mm strips


Electroplating copper tabs for battery packs


making of a short range electric skateboard battery pack
6s2p sony konion vtc6 with nickel plated copper 0.2 wide tabs


making of a lights battery pack from salvaged cells 2s3p


step by step diy triangle battery pack for electric bike


super cheap 10s battery for electric skateboard(also suitable for ebike)
Last edited by rojitor on Nov 21, 2017 5:32 pm, edited 12 times in total.

User avatar
Matador
10 kW
10 kW
Posts: 593
Joined: Jun 29, 2016 10:00 pm

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by Matador » Jun 23, 2017 11:54 am

Wow, inrush current so high you can se the wires twitch from the magnetic flux generated by the current flow.
Last edited by Matador on Jun 23, 2017 5:54 pm, edited 1 time in total.

User avatar
fechter
100 GW
100 GW
Posts: 12152
Joined: Dec 31, 2006 3:23 pm
Location: California Bay Area, USA

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by fechter » Jun 23, 2017 1:10 pm

Cool. I really like the one-handed electrode setup.
"One test is worth a thousand opinions"

User avatar
cal3thousand
10 GW
10 GW
Posts: 4054
Joined: Mar 26, 2012 4:47 pm
Location: California

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by cal3thousand » Jun 23, 2017 5:31 pm

This is quite a cool little device!! I love the small package, the soldering capability and the use of a 3S lipo (i have a ton of those).

Looks like this will be one of my next new toys/tools to incorporate. Thanks for taking the time to share this with us and write up a review. (I would never dare trying to post something like this on a Spanish-speaking site because my español is terrible; kudos to you)
Get a Cycle Analyst and a Multimeter, you're still a noob if you don't have at least one of each.

Planning on posting questions or buying anything on this site? Put up your country (at minimum) on your profile. This is a worldwide forum and we haven't reached clairvoyance.

User avatar
mxer
1 kW
1 kW
Posts: 346
Joined: May 15, 2011 9:01 am
Location: United Kindom

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by mxer » Jun 24, 2017 12:34 am

Looks super cool!!..

Lipo leads jump around a bit, I take it this is normal? 12vto35v so can be run on 6s as I have spares of them just not 3s..

Thanks for sharing top stuff!!!

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 24, 2017 3:52 pm

Yeah. No problem. The wires jumping is normal.
For the solder 12-35v is ok. Above 19v you get better performance.

cwah
10 GW
10 GW
Posts: 4483
Joined: Jul 24, 2011 5:42 am
Location: Between paris and london

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by cwah » Jun 24, 2017 5:57 pm

Wow cool

How much
Help me find my stolen electric brompton: http://bit.ly/1a0vbBC and Bosch Sinus B3 http://bit.ly/1eV0WQz

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 24, 2017 6:08 pm

Prices and instructions are at the end of my first post. You can check his blog too.

User avatar
tomjasz
1.21 GW
1.21 GW
Posts: 3737
Joined: Mar 29, 2014 1:45 pm
Location: Out riding, MN USA
Contact:

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by tomjasz » Jun 24, 2017 11:00 pm

rojitor wrote:Above 19v you get better performance.
So my 24v 18650 pack might be a good option?
Thanks Justin_le we're here thanks to you. All the best to the mods for their tireless work keeping it on an even keel.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 25, 2017 3:18 am

Yes. For the solder iron I am using a 25.2v charger I have around. Your 24v pack or a 6s lipo with an adapter will do.
I guess you can do some field job off the grid. That's the part I luv about this tiny thing.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 25, 2017 3:42 pm

I did a small soldering test.

Aulakiria
100 µW
100 µW
Posts: 8
Joined: Jun 25, 2017 11:18 pm

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by Aulakiria » Jun 25, 2017 11:23 pm

Please connect the soldering iron tip to the handle and turn on the power.
So the tip temperature is displayed correctly.

The soldering tip may occasionally have a different resistance value.
(Japanese Hakko original products and Chinese copy products)
Pressing the spot manual switch initializes the tip temperature info value.



A few people ordered according to your review.
I sent it today.

Thank you again for your review.

I recorded the orderer and tracking number.
http://blog.naver.com/aulakiria/221036236888

User avatar
tomjasz
1.21 GW
1.21 GW
Posts: 3737
Joined: Mar 29, 2014 1:45 pm
Location: Out riding, MN USA
Contact:

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by tomjasz » Jun 26, 2017 12:54 am

Sure would be nice to get more feedback!
Thanks Justin_le we're here thanks to you. All the best to the mods for their tireless work keeping it on an even keel.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 26, 2017 3:31 am

Hey! Welcome to the forum aulakiria.
When I watched my video I realized I have Turned it on before plugging the hakko. My bad. I know that's incorrect.
The solder at 25v works fine. I had really low expectations for 12v but it worked surprisingly well. It is a good choice for some off the grid field Jobs.
Your invention is boss!

Aulakiria
100 µW
100 µW
Posts: 8
Joined: Jun 25, 2017 11:18 pm

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by Aulakiria » Jun 26, 2017 3:41 am

Thank you. ^^

User avatar
jimwebo
10 W
10 W
Posts: 80
Joined: Mar 17, 2014 6:39 pm
Location: Asturias-North of Spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by jimwebo » Jun 26, 2017 4:07 am

Amazing.
Great job.
i need one these.
Electric life.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jun 28, 2017 11:49 am

I did a small video. How to use it. You can see how to navigate the menu.
enjoy

User avatar
sl33py
10 kW
10 kW
Posts: 697
Joined: Apr 24, 2015 5:21 pm
Location: Seattle, WA

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by sl33py » Jul 01, 2017 6:58 pm

Hey Aulakiria! Got your Boss spot welder just the other day and about to test.

I have more 4s packs than 3s... Can this use 4s Lipo instead of 3s? I'm charging an old 3s now, but not sure how long it'll last to be honest only a 25c 5000mAh zippy.

Fast shipping and seems really well made from first inspection!

User avatar
mxer
1 kW
1 kW
Posts: 346
Joined: May 15, 2011 9:01 am
Location: United Kindom

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by mxer » Jul 02, 2017 3:43 am

rojitor wrote:Yeah. No problem. The wires jumping is normal.
For the solder 12-35v is ok. Above 19v you get better performance.
mxer wrote:Looks super cool!!..

Lipo leads jump around a bit, I take it this is normal? 12vto35v so can be run on 6s as I have spares of them just not 3s..

Thanks for sharing top stuff!!!
I asked to use 6s for welding as I have no 3s and I think that was confirmed as a YES so 4s should be fine too.

The unit works from 12vto35v so should be fine but can't confirm 100%as I haven't received mine yet.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jul 02, 2017 4:14 am

No! That was for the solder. The solder works 12-35v
The spot welder 3s. They have different ports.

Image

A crappy 3s will work. It will need more time flux.
Also you can connect several 3s in parallel and you will have a perfect performance.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jul 02, 2017 4:21 am

It also works on 4s lipo.
However, the higher the voltage, the more dangerous it becomes.
High voltage causes metal deep penetration.
Spot welds of 18650 must be concentrated on the metal surface.
When the voltage increases, it is Arc welding.



The inside of the metal is melted. It damages the battery.
So try not to use 4s for the welder and definitely do not use 6s.

Aulakiria
100 µW
100 µW
Posts: 8
Joined: Jun 25, 2017 11:18 pm

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by Aulakiria » Jul 04, 2017 2:06 am

I introduce spot welding test results.
See http://blog.naver.com/aulakiria/221044436774.
I want you to do your battery and spot welding tests.

User avatar
rojitor
100 kW
100 kW
Posts: 1042
Joined: Mar 23, 2011 6:39 pm
Location: vigo spain

Re: BOSS LEVEL CUSTOM SPOT WELDER

Post by rojitor » Jul 07, 2017 1:52 pm

I installed a pedal today.
Image

It's easy to do. There's 3 wires com,normally open and normally closed. You need to solder com and normally closed to a dupont wire,insulate the third and you are done.
Dunno why the sellers send a tiny wire, I had to add an extension.
Image
also the diagram was incorrect. white,red and black were actually yellow,red and green...and red was not the supposed red. After a few combinations i figured it out.
I did a few welds and is quite comfortable.

Post Reply