Spot Welding Copper Strips to 18650 Battery Cells

Batteries, Chargers, and Battery Management Systems.
kdog   10 kW

10 kW
Posts: 685
Joined: Feb 02 2014 9:22pm
Location: hobart, tasmania

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by kdog » Aug 09 2020 2:00am

Hey garolittle
Whats the conductivity? IACS?
Cost? And where did you get it.
Cheers for info.

User avatar
garolittle   1 kW

1 kW
Posts: 440
Joined: Mar 03 2018 1:06pm
Location: Augusta, GA U.S.A

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by garolittle » Aug 09 2020 11:27am

serious_sam wrote:
Aug 08 2020 11:54pm
Those welds look really nice. I just looked into this material, but it appears to have a significantly higher resistance than all the other alternatives.

COPPER 1.7 x10^-6 Ω.cm
ALUMINIUM 2.6 x10^-6 Ω.cm
ZINC 6 x10^-6 Ω.cm
NICKEL 6.9 x10^-6 Ω.cm
IRON 9.7 x10^-6 Ω.cm
NICKEL-SILVER 28 x10^-6 Ω.cm

https://www.rfcafe.com/references/elect ... tivity.htm
https://calfinewire.com/datasheets/1001 ... vercda752/

EDIT: added second reference for nickel-silver resistivity
[/quote]

Correct. I apologize for not updating my post. I found out later that “Nickel Silver” does have a higher resistance so it would NOT be a good option for high current applications. I remember thinking “these welds are too good to be true”. Guess what? :oops:

User avatar
garolittle   1 kW

1 kW
Posts: 440
Joined: Mar 03 2018 1:06pm
Location: Augusta, GA U.S.A

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by garolittle » Aug 09 2020 11:28am

kdog wrote:
Aug 09 2020 2:00am
Hey garolittle
Whats the conductivity? IACS?
Cost? And where did you get it.
Cheers for info.
Hey Sir. I apologize for not updating my post. I found out later that “Nickel Silver” does have a higher resistance so it would NOT be a good option for high current applications.

User avatar
The Toecutter   10 kW

10 kW
Posts: 753
Joined: Feb 08 2015 4:02pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by The Toecutter » Aug 11 2020 12:55pm

I'm looking at ordering a spot welder. Is there anything cheap(< $300) out there capable of welding the following strip:

https://www.ebay.com/itm/133104900615?ul_noapp=true

I'd rather not experiment with building my own spot welder at this time as I just want to get this pack put together with minimal troubleshooting and get my project moving under battery power. I am using A123 26650 cells, and I am building a 24S4P pack of them. I plan to run them at 96A peak, and my BMS is rated for 100A pulse/50A cont.

If there is nothing appropriate within my price range, I'll probably have to go the DIY spot welder route, and delay getting my project running on batteries yet more.

User avatar
garolittle   1 kW

1 kW
Posts: 440
Joined: Mar 03 2018 1:06pm
Location: Augusta, GA U.S.A

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by garolittle » Aug 11 2020 5:00pm

Kweld is your best bet. About $200 USD

ossivirt   10 W

10 W
Posts: 90
Joined: May 18 2016 2:08pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by ossivirt » Aug 12 2020 1:32am

Kweld is probably best at that price point but 0.3mm copper could be too thick for it. Depends really how thick the nickel plating is on that strip. If you buy kweld for that job you want to go for dual lipos that will give close to 2000A weld current and thicker leads on electrodes to have any chance. Go take a look at the thread..

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Aug 12 2020 1:50am

:bigthumb: Good to know.
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan

User avatar
Merlin   10 MW

10 MW
Posts: 2081
Joined: Jan 29 2013 10:00am
Location: europe

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Merlin » Aug 13 2020 7:08am

no chance with kweld welding copper. i tried 0.1mm strips and doesnt work.

btw: you need a bit of resistance in your setup. if you go dual lipo with bigger wires your resistance is that low that you trip the 2000a limit easy.
that means it doesnt work if you wanna stay in warranty limits.

btw: the single 3s6000 graphene lipos do allready 1700A on setup. the 2nd in parallel is good for welding longer times. wires heat up way more than a single lipo.

for extended lifetime of your lipo i would recommend always 2 of them parallel or bigger ones like 3s16000

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11752
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by spinningmagnets » Aug 13 2020 7:20am

Merlin, have you tried the copper/nickel sandwich method. I highly recommend it for series connections.

0.20mm thick copper on the cells, and 0.15mm nickel over it. The nickel provides the resistance, and that size copper can easily handle 30A peaks, possibly more.

Copper is four times more conductive than nickel, so 0.20mm copper is equal to 0.80mm nickel...plus less heat.

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Aug 13 2020 8:41am

Interested because I'm either going to use .3mm copper / nickel coated spot welded, or just use plain soft copper and physically compression sandwich it like Kohlme did for his 26650 LiFePO4 pack.

I'd prefer welded. I think the positive terminals should be doable, but am concerned about the negative side blowing though. I've been saving junk AAs to practice on if/when I go the welded route.
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan

User avatar
Merlin   10 MW

10 MW
Posts: 2081
Joined: Jan 29 2013 10:00am
Location: europe

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Merlin » Aug 13 2020 9:28am

spinningmagnets wrote:
Aug 13 2020 7:20am
Merlin, have you tried the copper/nickel sandwich method. I highly recommend it for series connections.

0.20mm thick copper on the cells, and 0.15mm nickel over it. The nickel provides the resistance, and that size copper can easily handle 30A peaks, possibly more.

Copper is four times more conductive than nickel, so 0.20mm copper is equal to 0.80mm nickel...plus less heat.
not tried yet but interessting.
what kind of batteries do you build? i do 95% of all batteries with nickel sheets 0.2mm.(not strips)
for example surron packs 20s15p. those doing 300A battery current. i have temp sensors installed between, above and on +/- wire exits to monitor temps in real world usage.
whole pack with vtc6 is at 28mΩ. from specs i would miss the point of that extra work having 0.8mm nickel/0.2mm copper.

but of course evs/batteries in this smaller category cant run that massive amps continue. In real world usage i wouldnt talk about more than 20A continue for VTC6 without cooling solution.

less resistance is always nice but if the cells anyway heat up before just because of usage its hard to find the benefit of extra layers.
if i could use copper sheets i wouldnt go above 0.1mm because of the way better conductive material.

from experience even from those who ride their surrons at 50-60wh/km continue whole battery stays below 40°c. Thats pretty nice to me.

not sure even if could weld pure copper without nickel what happend overs years about humidity and copper inside a battery.

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Aug 13 2020 10:15am

Or... this approach looks very robust and easily made to carry the 350A surge current I'm designing for (borrowed from spiningmagnet's ebike site :D )

Spot weld the strips to the buss bar, then attach the strips to the cells.

Image
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11752
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by spinningmagnets » Aug 13 2020 10:49am

Using copper buses reduces voltage sag and waste-heat from the watts flowing through nickel. Of course, copper by itself cannot be welded onto a cell-end, so just put a 0.15mm nickel cap over it.

Try it on a bad cell, then check the resistance of a copper nickel sandwich, compared to thick nickel (0.25mm/0.30mm?)

The parallel connections can be pure nickel. Even 0.10 or 0.15 will work fine for paralleling.

User avatar
garolittle   1 kW

1 kW
Posts: 440
Joined: Mar 03 2018 1:06pm
Location: Augusta, GA U.S.A

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by garolittle » Aug 13 2020 12:45pm

hallkbrdz wrote:
Aug 13 2020 10:15am
Or... this approach looks very robust and easily made to carry the 350A surge current I'm designing for (borrowed from spiningmagnet's ebike site :D )

Spot weld the strips to the buss bar, then attach the strips to the cells.

Image
Nice! :D

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Aug 21 2020 8:33am

I assume the KWeld people are on holiday? Figures, finally have all the battery parts and nothing to assemble them with.

I'll be using 0.032 inch buss bars for the 4x5 groups with 0.08 inch bars for the 2x10 groups. That should prove adequate for my average current requirements along with 1/0 supply wires.
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Aug 24 2020 12:39pm

Wow. Great thread. Remind me never to go over to Facebook ES. It’s not the same professionalisms as here. Just my opinion......

I purchased 1,000 Tesla 2170 cells. 21700 ....
And I’m going to try my hand at a 4 or 5p 14s
Pack for my Framed Alaskan Fat Bike Build.

The other cells will be for a power wall or an EV car or Motorcycle....

I purchased the Kwelder..... I have 12v 9.6ah A123 LiFePO4 packs that do not voltage drop with a 5-7C load 45-65 amps.

How many Should I put in parallel for the Kwelder?
I’m sure each pack can peak at 200-400 amps

I’d like to do the Sandwich technique.
Is there another thread just on this???

Thank you.
http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Aug 24 2020 7:14pm

BTW - Keith said the KWeld kits won't be back in stock until the end of September. No details as to why.
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Aug 24 2020 7:18pm

hallkbrdz wrote:
Aug 24 2020 7:14pm
BTW - Keith said the KWeld kits won't be back in stock until the end of September. No details as to why.
mine has shipped :)
http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Aug 27 2020 7:00pm

I’d like to do the Sandwich technique.
Is there another thread just on this???

Thank you.

I have 21700 cells arrived today and the Kweld.
Now I need to wrap my head around the supply for the Kweld.
I have lots of 12.8 Nominal LiFePo4 9.6ah packs. at 45-65 amp draw, they maintain their voltage to 3.2v per parallel group within the packs(has jst's to monitor) I believe they can 250 or 400 CCA PB equivalent.

Kweld manual says 4-30V input 2,000 amp max so I'm thinking of putting two of my 12.8v nominal A123 9.6ah packs in series for 8s or 25.6V Nominal with still a CCA of 250 or 400. I might need to also run some more in Parallel too.

Any insight on using LiFePO4 on Kwelder????

Image
http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11752
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by spinningmagnets » Aug 28 2020 5:03pm

Discussion that is specific to the copper/nickel sandwich" method will now be moved to here:

"Copper/nickel sandwich buses for series connections"
viewtopic.php?f=14&t=108006

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Aug 29 2020 8:12am

spinningmagnets wrote:
Aug 28 2020 5:03pm
Discussion that is specific to the copper/nickel sandwich" method will now be moved to here:

"Copper/nickel sandwich" buses for series connections
viewtopic.php?f=14&t=108006
You are awesome!!!!!
http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
parabellum   10 MW

10 MW
Posts: 2085
Joined: Nov 19 2010 9:55am
Location: Dominican Republic, north.

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by parabellum » Aug 29 2020 4:47pm

Tommy L wrote:
Aug 27 2020 7:00pm

I
Kweld manual says 4-30V input 2,000 amp max so I'm thinking of putting two of my 12.8v nominal A123 9.6ah packs in series for 8s or 25.6V Nominal with still a CCA of 250 or 400. I might need to also run some more in Parallel too.

Any insight on using LiFePO4 on Kwelder????

Image
Do not go over 12v, start with 2 packs in parallel, those are 120A max cells, so you end up with 960A capable pack. Limitation will be the nickel connectors.
P. S. If those are cut 36v medical packs, filter out the block with the fuse weakened tab.

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Aug 30 2020 7:32am

parabellum wrote:
Aug 29 2020 4:47pm
Do not go over 12v, start with 2 packs in parallel, those are 120A max cells, so you end up with 960A capable pack. Limitation will be the nickel connectors.
P. S. If those are cut 36v medical packs, filter out the block with the fuse weakened tab.
My Pre-made packs are from 8-9 years ago. I believe the A123’s in them were 30amp max with a near zero volts @ that load individual cell test. I’m sure there’s a high resistance on the strips they used. But on my testing back then, no voltage drop pulling 5-7C on the pack. No speed drop over time use of the packs. I would just run Four or six or eight in series for what every i was running at the time. I used a 4 packs in series 51.2v nominal and 4 in parallel 38.4ah for a 2kw pack on my electric lawn tractor conversion. Zero voltage drop.

So I’ll start with two packs in parallel and see if it works. I might need four or eight in parallel.
I’ll just add one at a time.

I don’t want to over current the Kwelder either.
Just how will I know??? I do not want to blow it up. Lol. 🙏🏻🙏🏻🙏🏻🙏🏻

http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
Tommy L   100 kW

100 kW
Posts: 1121
Joined: Dec 23 2010 4:33pm
Location: Saint Augustine, Florida USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Tommy L » Sep 01 2020 9:50pm

Nickel under in center (simulate cell)
Then nickel on either side on top to create slit
with copper sandwich between.
90 joules 1200amps showing beautiful consistent
Spot welds with the Kwelder.
Very happy. 😁😊🙏🏻


Image

https://drive.google.com/file/d/19Fz66 ... p=drivesdk
http://www.rawvelocity.com

- 4th Hoolagan FS Mtn 9C-2810 with 128v nom 9.2ah A123 40S40P(1.2Kw) - Lyen 18Fet 4115 - 77.8kph :)
http://endless-sphere.com/forums/viewto ... =4&t=39480

- 3rd Catrike 700 Bionx PL350 Velo build
http://www.youtube.com/watch?v=rYdnkaAhVtI

- 2nd 150lbs Pusher Trailer
http://www.youtube.com/watch?v=Q1qTc4sjORY

- 1st Sears NS mtn bike - Rigid 10a drill 800rpm - 2 12v AGM - 1000 watt inverter - 600w dimmer for throttle, wicked torque!

48.2mph/77.8kph Club

User avatar
hallkbrdz   10 W

10 W
Posts: 99
Joined: Mar 24 2018 1:47pm
Location: Edmond, OK USA

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by hallkbrdz » Sep 02 2020 8:31am

Good to know. I picked up my batteries and will try it out tonight on some scrap copper.
EKartGo - Building a kart for 100cc TAG competition :es:
ES thread viewtopic.php?f=34&t=107963
KartPulse thread https://forums.kartpulse.com/t/ekartgo-project/5857/1
Bryan