Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 08 2017 12:19pm

Hi guys!
I've got a Boston-Power Swing 5300 cell tested and want to share the results with you.
[+] About Boston-Power
Boston-Power is a US based manufacturer of Li-ion cells which makes them in China and Taiwan and supplies to HP, ASUS and EV makers.
The cell was bought from Queen Battery, a Chinese supplier of genuine batteries, who specializes mainly on EV and eBike market. Queen Battery has a branch in Europe which works with european customers like me:)

The Boston-Power Swing 5300 is a 3.65V Li-ion cell with a wide working temperature range (-40 to +70°C).
Image
Image

Specs taken out of it's datasheet:

Nominal capacity: 5300mAh (at 0.2C discharge)
Nominal energy: 19.3Wh (at 0.2C discharge)
Nominal cell impedance: 16 mΩ
Life cycle at 100% DOD: >1000 cycles (at 1C discharge)
Discharge cut-off voltage: 2.75V
Max continuous discharge rate: 13A
Standard charging current: 3.7A, cut-off at 0.05A
Max continuous charge rate: 10.6A
Weight: 93g
Charging temperature: -20 to +60°C
Discharging temperature: -40 to +70°C
Dimensions: 37.2 x 64.8 x 19.1mm

I've tested with ZKETECH EBC-A20 and a self-made battery holder. It's a PC-connected battery tester supporting 4-wire measuring and discharging at up to 20A.
Image
I've tried to follow all the prescriptions of the IEC61960-2003 standard concerning battery's capacity measurement. Before each discharging cycle the battery was charged at 3.7A to 4.2V (cut-off at 0.1A, which is higher than 0.05A allowed by the manufacturer, but it's the lowest supported by EBC-A20). Before each discharging or charging i've held a 1-1.5hrs pause. The environment temperature was 21-23°C.

Discharge cut-off voltage was 2.75V in all cases. I've done a 0.2C (1.06A) discharging to check the nominal capacity, then I've discharged at 5.0 and 10.0A and finished with the max allowed continuous discharge current - 13A.

The results i've grouped together, so it must be easier to compare them.
Image

As turned out, the battery is not overrated and at 0.2C it gives out 5318mAh - a lil bit more than the nominal capacity. The amount of energy is also slightly higher than the nominal - 19.36 vs 19.3Wh.

At 5.0A the capacity is lower than at 10.0A, but the amount of energy is higher. This is a normal thing, and the important one is the amount of energy.

At 13.0A the measured capacity was 5091mAh and the energy - 16.48Wh.

The results are good and not surprising for me. This is a high quality cell which can give out almost 5100mAh/16.5Wh at 13.0A. In some cases the prismatic form is preferable than cylindrical and i think it will help to build battery packs with higher energy density than in case of using 26650 cells with ~5000mAh capacity.

P.S. This is my first post on Endless-sphere and i hope not the last :) Please tell me what do you think about this review/test, what did you like or didn't like and would you like to see tests of other batteries done in similar way?
Last edited by thunderheart on Aug 16 2019 5:21pm, edited 1 time in total.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

999zip999   100 GW

100 GW
Posts: 9460
Joined: Jan 10 2010 1:40pm
Location: Dana Point So. Cal

Re: Boston-Power Swing 5300 Li-ion cell test

Post by 999zip999 » Oct 08 2017 12:44pm

Thank you always looking for the next great battery. Plus I like the 4 wire battery tester. Now the question how much are these cells ? Welcome to E.S.

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 08 2017 12:58pm

999zip999 wrote:Thank you always looking for the next great battery. Welcome to E.S.
Thanks for warm welcome!:)
999zip999 wrote:Now the question how much are these cells ?
Queen Battery sells them at US$ 2.6 plus shipping or US$ 5.3 (100pcs/lot) or US$ 5.7 (30pcs/lot) with free shipping to USA/Europe (UPS, FedEx, etc...), but it's possible to have a personal discount depending on the quantity/total price of your order. They are very customer-friendly:) They helped me to avoid european import taxes by sending the batteries from their EU branch.
Last edited by thunderheart on Oct 08 2017 6:41pm, edited 1 time in total.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

Hillhater   100 GW

100 GW
Posts: 10914
Joined: Aug 03 2010 10:33pm
Location: Sydney ..(Hilly part !) .. Australia/ Down under !

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Hillhater » Oct 08 2017 6:04pm

It still looks suspicously like a pair of 18650s assembled in parallel ?
Pull the shrinkwrap off and let us see what is inside . :wink:
This forum owes its existence to Justin of ebikes.ca

User avatar
amberwolf   100 GW

100 GW
Posts: 30469
Joined: Aug 17 2009 6:43am
Location: Phoenix, AZ, USA, Earth, Sol, Local Bubble, Orion Arm, Milky Way, Local Group
Contact:

Re: Boston-Power Swing 5300 Li-ion cell test

Post by amberwolf » Oct 09 2017 1:13am

Hillhater wrote:It still looks suspicously like a pair of 18650s assembled in parallel ?
Pull the shrinkwrap off and let us see what is inside . :wink:
According to your own posts and the image you linked in this thread from a few months ago:
https://endless-sphere.com/forums/viewt ... 14&t=89482
they're not. ;)


There's also an older thread
https://endless-sphere.com/forums/viewt ... 31&t=81815
that actually has a pic of one cut open

Hillhater   100 GW

100 GW
Posts: 10914
Joined: Aug 03 2010 10:33pm
Location: Sydney ..(Hilly part !) .. Australia/ Down under !

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Hillhater » Oct 09 2017 5:20am

I had not seen the internals previously...thats why i was still suspicous !
This forum owes its existence to Justin of ebikes.ca

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 09 2017 6:54am

Hillhater wrote:It still looks suspicously like a pair of 18650s assembled in parallel ?
No :)
Image
Image
Image
Image
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

Hillhater   100 GW

100 GW
Posts: 10914
Joined: Aug 03 2010 10:33pm
Location: Sydney ..(Hilly part !) .. Australia/ Down under !

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Hillhater » Oct 09 2017 8:24pm

Yes , i have seen similiar "unrapped" pictures before, but even there it still looks "suspiciously like". A pair of 18650s in a metal case.!
But AW linked to a post with the can cut open to prove it is a single , oval wound, cell construction.
Its basic performance specs are not outstanding by current standards, but maybe it has some advantage in cycle life, safety, US availability, etc ?????
This forum owes its existence to Justin of ebikes.ca

cheapcookie   100 W

100 W
Posts: 190
Joined: Aug 02 2014 10:34pm
Location: Earth

Re: Boston-Power Swing 5300 Li-ion cell test

Post by cheapcookie » Oct 10 2017 1:28am

It has incredible belgian chocolate in it ... :wink:

Pajda   1 kW

1 kW
Posts: 344
Joined: Jan 24 2016 3:45am
Location: Czech Republic

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Pajda » Oct 10 2017 1:34am

It seems that they have outstanding temperature operation range. Maybe the best on the market of cells with C(Si) anode. At least according to the datasheet.

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 10 2017 6:05am

cheapcookie wrote:It has incredible belgian chocolate in it ... :wink:
And Belgian beer as electrolyte :)
Pajda wrote:It seems that they have outstanding temperature operation range
And incredible life cycle, even at 100%DOD
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

redilast   1 kW

1 kW
Posts: 317
Joined: Apr 14 2016 12:47am

Re: Boston-Power Swing 5300 Li-ion cell test

Post by redilast » Oct 11 2017 12:49am

I have some of these laying around in an old medical device pack. It's got like 12 of these inside.

The cycle life claims are most intriguing, but are the claims true? Cycling these 1000 times or so sure would take a while.

Also I like the holders that are available for these cells. Could make for some pretty well put together packs!
Last edited by redilast on Oct 11 2017 2:04am, edited 1 time in total.

User avatar
DrkAngel   100 GW

100 GW
Posts: 5332
Joined: Dec 15 2010 11:14am
Location: Upstate-Western-Southern Tier NY. USA

Re: Boston-Power Swing 5300 Li-ion cell test

Post by DrkAngel » Oct 11 2017 1:57am

.
...
Sonata version $2.80 - $3.75 per cell

Cells in 3s5p (15 pcs) "packs" ... "used for 9 months"

Boston Power 5300 "Sonata" specs (pdf) - 1.5C charge 1.5C+ continuous discharge

Boston Power 5300 "Swing" specs (pdf) - 2C charge <2.5C continuous discharge

Dramatic claims, most impressive that I've seen, that DOD is major factor in cycle life!

Image
Attachments
Swing 5300.jpg
Swing 5300.jpg (133.22 KiB) Viewed 10622 times
A little learning is a dangerous thing;
Drink deep, or taste not the Pierian spring:
There, shallow draughts intoxicate the brain,
And drinking largely, sobers us again.

I enjoy enlightening ... and enlivening the spirit of the innovators.

New & Improved - Acronym Definitions

Index - Homemade Battery Packs - Updated - December 2019

EBike Toolbox - Bargains! $

Endless Sphere Wiki - Lost?

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 11 2017 10:00am

redilast wrote:I have some of these laying around in an old medical device pack.
Could you give more info about that medical device please?
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

User avatar
shinyballs   1 kW

1 kW
Posts: 323
Joined: Sep 29 2007 2:43am
Location: WA, USA

Re: Boston-Power Swing 5300 Li-ion cell test

Post by shinyballs » Oct 12 2017 4:59pm

What's the recommended way to connect the cells? Can you just spot weld the ends using .15mm nickel?
Thanks for sharing your test results.
Sale section etiquette, pls be courteous to other members, if you know of a better deal or do not agree with the sale price, do not shove links to similar products being sold by someone else in another member's post.. it's just not nice. If you suspect a scam pls FLAG the thread for moderation and it will be checked out... i know this is a tough one to call but put yourself in the seller's shoes and imagine how you would like it.

http://endless-sphere.com/forums/viewto ... 31&t=25446

youyoung21147   100 mW

100 mW
Posts: 41
Joined: Jul 21 2016 5:14am

Re: Boston-Power Swing 5300 Li-ion cell test

Post by youyoung21147 » Oct 13 2017 7:02am

Nice to see they have 2 flat sides ! Makes the pack more energy dense per unit volume and also easier to liquid cool !

Also the vent notch on side is a cool safety feature, at least the sidewall failure location is predictable. But the inside visible in this post :

https://endless-sphere.com/forums/viewt ... 31&t=81815

OMG that looks so messy ! The inside of a cylindrical cell inspires much more confidence with no kink zone whatsoever and perfectly wrapped material... Would be curious to see how a big batch of this cell survives abuse

LanH   1 µW

1 µW
Posts: 2
Joined: Mar 24 2017 11:14am

Re: Boston-Power Swing 5300 Li-ion cell test

Post by LanH » Oct 13 2017 7:55am

Thank you for this useful results.

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 13 2017 4:37pm

shinyballs wrote:What's the recommended way to connect the cells? Can you just spot weld the ends using .15mm nickel?
No idea. hemo says they are hard to weld.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

hemo   100 W

100 W
Posts: 197
Joined: Mar 30 2016 5:13pm
Location: England, GB ( UK).

Re: Boston-Power Swing 5300 Li-ion cell test

Post by hemo » Oct 17 2017 1:24pm

The cells are hard to tab weld and the ends are as hard as nails apparently. They were conceived to work with a modular set up/connection, which I believe in themselves are not cheap to buy.
Jimmy the boss at Insat Intl/ BGA Reworking in North London has boxes and boxes of these in his work space, and tab welds using copper. His normal industrial spot welder couldn't manage decent welds to the Boston's, so in order to accomplish this he said his new state of the art welder cost about 30k sterling.
Might be interesting to see if any one buys these and whether they are able to manage welding them or not.

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Boston-Power Swing 5300 Li-ion cell test

Post by thunderheart » Oct 17 2017 7:05pm

hemo, thanks for info. It's very important, i think.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11645
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Boston-Power Swing 5300 Li-ion cell test

Post by spinningmagnets » Mar 05 2018 11:55am

Here's the best video showing the insides of the Boston Power style of cells, with the insides being "oval" wound, instead of cylindrical. Fast forward to the 9:44 mark...

https://youtu.be/TNk0bouiPDQ?t=586


Headrc   100 W

100 W
Posts: 164
Joined: Aug 11 2015 2:09am

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Headrc » Mar 10 2018 9:48am

Excellent review here on this battery. Has anyone since tried welding any of these? I corresponded with the gent who did that review on Youtube and was told problem soldering them just like 18650s ...so I would think they could be spot welded just as easily.

Pajda   1 kW

1 kW
Posts: 344
Joined: Jan 24 2016 3:45am
Location: Czech Republic

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Pajda » Mar 10 2018 4:57pm

Yes they could be easily spot welded by cheap Chinese welders as for example LG HG2 cells.

.. edited for writing nosenses :oops:
Last edited by Pajda on Mar 11 2018 6:28am, edited 1 time in total.

Hillhater   100 GW

100 GW
Posts: 10914
Joined: Aug 03 2010 10:33pm
Location: Sydney ..(Hilly part !) .. Australia/ Down under !

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Hillhater » Mar 11 2018 1:25am

Pajda wrote:
Mar 10 2018 4:57pm
Yes they could be easily spot welded ......
...... Their housing is made from aluminium as on most 18650 cells.
:shock: Every 18650 i have seen had a steel case ....(magnetic) !.
This forum owes its existence to Justin of ebikes.ca

Pajda   1 kW

1 kW
Posts: 344
Joined: Jan 24 2016 3:45am
Location: Czech Republic

Re: Boston-Power Swing 5300 Li-ion cell test

Post by Pajda » Mar 11 2018 6:33am

You are right that 18650 cells are in steel cese. I found one datasheet for Boston Swing 5300 with info that their casing is made from aluminium. But I did not checked that. Anyway I have no problem with welding nickel tabs on Swing 5300 with the same setting as on 18650 cells.

Post Reply