Panasonic NCR18650BD 3200mAh 10A cell's capacity test

Batteries, Chargers, and Battery Management Systems.
Post Reply
User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Panasonic NCR18650BD 3200mAh 10A cell's capacity test

Post by thunderheart » May 03 2019 5:15am

Panasonic NCR18650BD is a mid-drain high capacity Li-ion cell in traditional 18650 format. It's rated at 3180mAh and supports discharging at up to 10A.
Image

The battery was bought from my reliable supplier (Queen Battery) and tested with ZKETECH EBC-A20 and a self-made battery holder. It's a PC-connected battery tester supporting 4-wire measuring and discharging at up to 20A.
Image

I've used version 3.0 of my battery holder based on 0.5mm thick pure copper terminals
Image
Image

I've followed all the prescriptions of the IEC61960-2003 standard concerning battery's capacity measurement. Before each discharging cycle each battery was charged at standard charge current mentioned in its datasheet to charge end voltage. Before each discharging or charging i've held a 1-1.5hrs pause. The environment temperature was 23.0-24.5°C. To be sure in results i've done each test minimum twice (usually 3-4 times).


Panasonic NCR18650BD

My cell has the following marking: C CV 7321.
Image

Specifications from NCR18650BD datasheet:
Rated capacity: 2980mAh at 20°C
Minimum capacity: 3030mAh at 25°C
Typical capacity: 3180mAh at 25°C
Nominal voltage: 3.6V
Standard charge current: 0.909A (0.3C)
Max charge current: 1.5A
Charge end voltage: 4.20V
Charge cut-off current: 60.6mA (0.02C) (100mA used)
Max continuous discharge current: 10A
Discharge cut-off voltage: 2.5V
AC impedance at 1KHz: ≤35mΩ
Max weight: 49.5g

The measured weight of my cell is 46.66g. Measured DCIR at 3030mAh was 23.8±1.0mΩ (in fully charged condition).
Image

NCR18650BD capacity test results:
Image
At 0.2C or 0.61A NCR18650BD's capacity was a bit higher than declared and it didn't go below 3020mAh all the way up to 10A. The curves look excellent even at 10A. Just a great cell, nothing to add.

Here is the video version of this review
Image


Check out my YouTube channel for batteries, chargers and other stuff reviews.
I've launched my blog where you can find all my reviews in one place. Every new test/review will be first published on YouTube and in the blog. I'll be happy to see new subscribers, comments, suggestions and just your thoughts.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

la8rat   1 W

1 W
Posts: 59
Joined: Mar 12 2019 10:34am

Re: Panasonic NCR18650BD 3200mAh 10A cell's capacity test

Post by la8rat » May 03 2019 5:40am

:bigthumb:

Joachim   1 kW

1 kW
Posts: 435
Joined: Jul 30 2015 1:02pm
Contact:

Re: Panasonic NCR18650BD 3200mAh 10A cell's capacity test

Post by Joachim » May 03 2019 7:56am

Why discharge to 2.5Volt ? they never get 300 to 500 cycles 20/30% los....more like 50/60%

Not bad for cells from march 2017