Post by fechter » Feb 21 2019 2:46pm

That's strange then.

About the only other things that come to mind are using enough pressure on the electrodes, making sure the nickel surface is clean and free of any contaminants (like oil), and maybe the electrode material. I use solid copper wire for electrodes on mine and get great results with .15 nickel, but I have not tried 0.2 nickel.
"One test is worth a thousand opinions"

User avatar
Cowardlyduck   10 MW

10 MW
Posts: 2465
Joined: Jun 26 2011 8:41pm
Location: Canberra, ACT, Australia

Re: JP spot welder

Post by Cowardlyduck » Feb 22 2019 4:48am

I've had good success with this seller:
https://www.aliexpress.com/item/18650-L ... c4dOjccJ1
Still using a 1kg roll of 0.15 x 7mm I bought several years ago (nearly used it all now), and I just ordered a new roll of 0.15 x 8mm that's yet to arrive.

They have 0.2 x 10mm rolls for a decent price. :)

Cheers
High Power LiPo wiring harnesses - 4P - XT90, HXT4mm, 5.5mm. 200Amp+ capable. Global shipping.

Modified Stealth Fighter - Force air cooled motor @ 6KW, Adaptto Mini-E. 49AH, 52V 18650 - 2.5Kwhr
Cowardlyducks - Stealth Fighter Videos

BikeE recumbent commuter - 9C, 6Fet Grinfineon, internal 17AH, 52V, + on-board solar.

Ebike Garage - My YouTube Ebike ramblings.

User avatar
Offroader   10 MW

10 MW
Posts: 2300
Joined: Sep 08 2013 9:03pm
Location: USA

Re: JP spot welder

Post by Offroader » Feb 22 2019 6:56pm

Cowardlyduck wrote:
Feb 22 2019 4:48am
I've had good success with this seller:
https://www.aliexpress.com/item/18650-L ... c4dOjccJ1
Still using a 1kg roll of 0.15 x 7mm I bought several years ago (nearly used it all now), and I just ordered a new roll of 0.15 x 8mm that's yet to arrive.

They have 0.2 x 10mm rolls for a decent price. :)

Cheers
Did you test the nickel to make sure its 100%, with grinding or salt water? pretty much all of the nickel you buy will be fake and unless you test it you won't know.

User avatar
Cowardlyduck   10 MW

10 MW
Posts: 2465
Joined: Jun 26 2011 8:41pm
Location: Canberra, ACT, Australia

Re: JP spot welder

Post by Cowardlyduck » Feb 22 2019 8:18pm

Offroader wrote:
Feb 22 2019 6:56pm
Did you test the nickel to make sure its 100%, with grinding or salt water? pretty much all of the nickel you buy will be fake and unless you test it you won't know.
Yes, tested by scraping and leaving in salt water over night. I wouldn't have built 4 packs from this roll already if I wasn't sure it is pure nickel.

Cheers
High Power LiPo wiring harnesses - 4P - XT90, HXT4mm, 5.5mm. 200Amp+ capable. Global shipping.

Modified Stealth Fighter - Force air cooled motor @ 6KW, Adaptto Mini-E. 49AH, 52V 18650 - 2.5Kwhr
Cowardlyducks - Stealth Fighter Videos

BikeE recumbent commuter - 9C, 6Fet Grinfineon, internal 17AH, 52V, + on-board solar.

Ebike Garage - My YouTube Ebike ramblings.

ALLVLTS   10 mW

10 mW
Posts: 23
Joined: May 10 2012 11:18am
Location: MD, USA

Re: JP spot welder

Post by ALLVLTS » Feb 23 2019 2:30pm

Hi ES,
I hope everyone is doing well.
It's been a long time but I finally just set up the new JP spot welder I bought last year (health issues always get in the way of fun), and I think I fried something. Could be a couple causes.

12V battery is an Optima Redtop, 720 CCA, 4.5 years old though pulled from my SUV still working fine. Should be good for this.
I hooked everything up properly but of course slipped and arced the wrench between the battery terminals on the last bolt (shouldn't play with power while sleep deprived... but hard to realize that while sleep deprived!). I was hoping that it didn't do anything to the welder since it wasn't shorted *through* the welder, but the negative terminal was connected at that point (not the 12V power supply yet, though).

I finished setting up then tried to weld a salvaged nickel strip onto an old (fully discharged) 18650 to practice. Nothing happened. The pot was turned all the way CCW, so I turned it CW to about 25% and tried again. When I hit the pedal I got full battery power and it vaporized the nickel and put a crater into the cell... Huge pop and sparks. I should have stopped and troubleshot right there, but still not thinking straight, I turned it all the way back CCW and tried again. This time as soon as the leads touched the cell, BAM, full battery power and huge sparks again *WITHOUT* touching the pedal. Yikes! I stopped there and put a voltmeter on the leads, had full batt voltage (12.8V). It was then that I noticed my 12V power supply had an intermittent connection, so that may have had something to do with it?

I disconnected the power supply and the pedal, and STILL had full voltage between the leads. I pulled the welder off the battery and checked continuity between the connection points and had some resistance, increasing with time (as if a cap were charging). I put it away then and waited for a new 12V power supply. Couple days later, there was a high resistance between the leads (didn't think to record the resistance... still sleeping very badly).

Reconnected to the battery, checked voltage again. It started at about 9 volts then worked its way up to 12.8 over a minute or so without any input (wth?). I plugged in the new 12V PS to see if it changed anything... nope. After reading over this entire thread again I realized I hadn't checked or seen the green LED, so I plugged in the pedal and pressed then saw 2 flashes. Increasing the pot increased the brightness of the flashes, so I feel like that part is working.

On page 37 of this thread it was mentioned that a similar failure had meant one of 3 things... Bad PIC, bad mosfet driver, or blown mosfets. Given the novella I just wrote, can anyone tell me how to determine where the fault lies? Whatever it is, I can replace it as a part of my job is to install or replace PCA components, I just don't know how to troubleshoot this one further.

Jakov, if it is a damaged PIC, do you have a new one that I can purchase from you at this time?

Thanks, all.

User avatar
fechter   100 GW

100 GW
Posts: 13260
Joined: Dec 31 2006 3:23pm
Location: California Bay Area, USA

Re: JP spot welder

Post by fechter » Feb 23 2019 5:56pm

Sounds like you blew the MOSFETs. It's a good sign if the LED still blinks.
"One test is worth a thousand opinions"

NetPro   10 mW

10 mW
Posts: 29
Joined: Oct 09 2015 2:52pm
Location: USA

Re: JP spot welder

Post by NetPro » Feb 23 2019 10:58pm

Cowardlyduck wrote:
Feb 22 2019 4:48am
I've had good success with this seller:
https://www.aliexpress.com/item/18650-L ... c4dOjccJ1
Still using a 1kg roll of 0.15 x 7mm I bought several years ago (nearly used it all now), and I just ordered a new roll of 0.15 x 8mm that's yet to arrive.

They have 0.2 x 10mm rolls for a decent price. :)

Cheers
Very good. That is what I was looking for.
If the 0.15 sold by that merchant was good stuff, as you have confirmed, I am willing to take a chance on his 0.20 stock and see if bad nickel strips is the reason for sticking electrodes.
I have placed an order and will report once I get it.

Thanks a bunch!

NetPro   10 mW

10 mW
Posts: 29
Joined: Oct 09 2015 2:52pm
Location: USA

Re: JP spot welder

Post by NetPro » Feb 23 2019 11:17pm

fechter wrote:
Feb 21 2019 2:46pm
That's strange then.

About the only other things that come to mind are using enough pressure on the electrodes, making sure the nickel surface is clean and free of any contaminants (like oil), and maybe the electrode material. I use solid copper wire for electrodes on mine and get great results with .15 nickel, but I have not tried 0.2 nickel.
I am surprised solid copper wire works for you. I have never tried because I read somewhere that annealed copper wasn't good for electrodes.
I will try AWG 10 and 12 and see what I get.
Using this gizmo I built (welding head) allows me to adjust the spring tension from very light to very, very strong.
I have tried the entire scale with different welders, set at different voltages and current inputs and using different brands of scrap batteries for testing.
Maybe using solid copper wire does the trick. Easy enough to test. . . .

User avatar
Cowardlyduck   10 MW

10 MW
Posts: 2465
Joined: Jun 26 2011 8:41pm
Location: Canberra, ACT, Australia

Re: JP spot welder

Post by Cowardlyduck » Feb 25 2019 6:39am

NetPro wrote:
Feb 23 2019 10:58pm
Very good. That is what I was looking for.
If the 0.15 sold by that merchant was good stuff, as you have confirmed, I am willing to take a chance on his 0.20 stock and see if bad nickel strips is the reason for sticking electrodes.
I have placed an order and will report once I get it.

Thanks a bunch!
No worries :)

On a different note, I've never been a huge fan of the large copper tips supplied with my JP. They do the job, but make pinpoint close welds difficult.
I prefer a much smaller point at the end so I tried various things like filing, grinding with a dremel, but nothing I tried was very quick or easy.

So I came up with this idea...why not use a steel pencil sharpener:
DSC_5251.JPG
After a bit of effort:
DSC_5252.JPG
I started by hand but that quickly got old and started to hurt my hand.

So instead I switch to automatic mode :D
DSC_5253.JPG
The results speak for themselves:
DSC_5255.JPG
Only downside is the mess and slight loss of copper...but the lost copper was not usable anyway.
DSC_5257.JPG
I recommend holding the sharpener tight with some pliers though...I found out the hard way what happens when it catches and spins in your hand. :lol:

Testing has proven successful with a bunch of welds doing very well and I can now much more easily manoeuvre the tips. :)

Cheers
High Power LiPo wiring harnesses - 4P - XT90, HXT4mm, 5.5mm. 200Amp+ capable. Global shipping.

Modified Stealth Fighter - Force air cooled motor @ 6KW, Adaptto Mini-E. 49AH, 52V 18650 - 2.5Kwhr
Cowardlyducks - Stealth Fighter Videos

BikeE recumbent commuter - 9C, 6Fet Grinfineon, internal 17AH, 52V, + on-board solar.

Ebike Garage - My YouTube Ebike ramblings.

NetPro   10 mW

10 mW
Posts: 29
Joined: Oct 09 2015 2:52pm
Location: USA

Re: JP spot welder

Post by NetPro » Feb 25 2019 10:01am

Cowardlyduck wrote:
Feb 25 2019 6:39am

No worries :)

On a different note, I've never been a huge fan of the large copper tips supplied with my JP. They do the job, but make pinpoint close welds difficult.
I prefer a much smaller point at the end so I tried various things like filing, grinding with a dremel, but nothing I tried was very quick or easy.

So I came up with this idea...why not use a steel pencil sharpener:
DSC_5251.JPG
After a bit of effort:
DSC_5252.JPG
I started by hand but that quickly got old and started to hurt my hand.

So instead I switch to automatic mode :D
DSC_5253.JPG

The results speak for themselves:
DSC_5255.JPG

Only downside is the mess and slight loss of copper...but the lost copper was not usable anyway.
DSC_5257.JPG
I recommend holding the sharpener tight with some pliers though...I found out the hard way what happens when it catches and spins in your hand. :lol:

Testing has proven successful with a bunch of welds doing very well and I can now much more easily manoeuvre the tips. :)

Cheers
Using a pencil sharpener to re-dress the electrode tips is an excellent tip :bigthumb:

Not sure how long the blades that come with the sharpeners will last though, specially with the hard copper of which some electrodes are made. (I have a couple of them from different sources and some are harder than others)

But how about this :idea:
Buy a diamond sharpening card, cut a piece using the steel blade as a template and replace the stock one (face down, or course).
These sharpeners are very long lasting, come in different grits and might work well for this purpose.
If it works, beats having to mount the electrodes in the lathe and doing all the setup required to do this kind of work.

Great tip!

User avatar
fechter   100 GW

100 GW
Posts: 13260
Joined: Dec 31 2006 3:23pm
Location: California Bay Area, USA

Re: JP spot welder

Post by fechter » Feb 25 2019 2:00pm

I did something similar only used my bench grinder instead of a pencil sharpener. Spin the electrode with a drill and hold at an angle against the grinder while it is running. Makes fast work of it but not a super smooth finish.
"One test is worth a thousand opinions"

ALLVLTS   10 mW

10 mW
Posts: 23
Joined: May 10 2012 11:18am
Location: MD, USA

Re: JP spot welder

Post by ALLVLTS » Feb 27 2019 11:31am

fechter wrote:
Feb 23 2019 5:56pm
Sounds like you blew the MOSFETs. It's a good sign if the LED still blinks.
Thanks for the input. Any way to test them without removing them?

User avatar
fechter   100 GW

100 GW
Posts: 13260
Joined: Dec 31 2006 3:23pm
Location: California Bay Area, USA

Re: JP spot welder

Post by fechter » Feb 27 2019 12:37pm

ALLVLTS wrote:
Feb 27 2019 11:31am
Thanks for the input. Any way to test them without removing them?
You can use an ohmmeter to measure across the drain to source but since they are all in parallel, if any one shorts, you can't easily tell which one it was without removing them.
"One test is worth a thousand opinions"

ALLVLTS   10 mW

10 mW
Posts: 23
Joined: May 10 2012 11:18am
Location: MD, USA

Re: JP spot welder

Post by ALLVLTS » Feb 27 2019 1:35pm

Okay, that's certainly better than nothing... I'll check them out. If any of them are bad then I'd prefer to replace all of them anyway (then I can find out which were bad just because I'm curious). Thanks again.

User avatar
fechter   100 GW

100 GW
Posts: 13260
Joined: Dec 31 2006 3:23pm
Location: California Bay Area, USA

Re: JP spot welder

Post by fechter » Feb 28 2019 9:21am

ALLVLTS wrote:
Feb 27 2019 1:35pm
Okay, that's certainly better than nothing... I'll check them out. If any of them are bad then I'd prefer to replace all of them anyway (then I can find out which were bad just because I'm curious). Thanks again.
Yes, that's a good plan. Replace all of them with parts from the same batch.
"One test is worth a thousand opinions"

NetPro   10 mW

10 mW
Posts: 29
Joined: Oct 09 2015 2:52pm
Location: USA

Re: JP spot welder

Post by NetPro » Mar 06 2019 3:03pm

NetPro wrote:
Feb 23 2019 10:58pm
Cowardlyduck wrote:
Feb 22 2019 4:48am
I've had good success with this seller:
https://www.aliexpress.com/item/18650-L ... c4dOjccJ1
Still using a 1kg roll of 0.15 x 7mm I bought several years ago (nearly used it all now), and I just ordered a new roll of 0.15 x 8mm that's yet to arrive.

They have 0.2 x 10mm rolls for a decent price. :)

Cheers
Very good. That is what I was looking for.
If the 0.15 sold by that merchant was good stuff, as you have confirmed, I am willing to take a chance on his 0.20 stock and see if bad nickel strips is the reason for sticking electrodes.
I have placed an order and will report once I get it.

Thanks a bunch!
The 0.20 nickel arrived a few days ago and I am happy to report it appears to be the real thing.
I first folded over a couple a piece about 2 inches long and took it to the grinder.
Though, I saw a couple of little sparks here and there, it was pretty much spark-free, when compared to a known nickel-plated ribbon.

So, sanded down about 0.05 on each side and put it in water with table salt for three days now and I don't see ANY rust whatsoever.
By the way, high quality Brown & Sharphe micrometer confirms 0.20 MM for the thickness.
As far as how it welds, if using the kWeld welder with the thick electrodes it comes with, pretty darn good.

Using any other electrodes, my forever-going sicking problem is still there. In any case, I can get a properly formed nugget when I adjust electrode pressure and the current and/or time carefully.

User avatar
Cowardlyduck   10 MW

10 MW
Posts: 2465
Joined: Jun 26 2011 8:41pm
Location: Canberra, ACT, Australia

Re: JP spot welder

Post by Cowardlyduck » Mar 07 2019 4:20am

NetPro wrote:
Mar 06 2019 3:03pm
The 0.20 nickel arrived a few days ago and I am happy to report it appears to be the real thing.
I first folded over a couple a piece about 2 inches long and took it to the grinder.
Though, I saw a couple of little sparks here and there, it was pretty much spark-free, when compared to a known nickel-plated ribbon.

So, sanded down about 0.05 on each side and put it in water with table salt for three days now and I don't see ANY rust whatsoever.
By the way, high quality Brown & Sharphe micrometer confirms 0.20 MM for the thickness.
As far as how it welds, if using the kWeld welder with the thick electrodes it comes with, pretty darn good.

Using any other electrodes, my forever-going sicking problem is still there. In any case, I can get a properly formed nugget when I adjust electrode pressure and the current and/or time carefully.
Awesome!
Yeah, I can also report that (for the second time now) this seller has legit pure nickel. I did the same salt water test, and then promptly forgot about it for a week...if it doesn't rust after a week it aint gonna.
Here is my result:
DSC_5258.JPG
DSC_5258.JPG (71.14 KiB) Viewed 147 times
DSC_5259.JPG
DSC_5259.JPG (59.32 KiB) Viewed 147 times
The brown stuff in the water is from the salt I used...only salt I could find at the time was Himalayan rock salt. :lol:

Haven't measured the thickness, but it is about 1mm wider than the 7mm stuff I got last time, so spot on since this time I ordered 8mm wide.

I was hoping for 0.2x8mm stuff, but it seems this was the one size they didn't have.

Cheers
High Power LiPo wiring harnesses - 4P - XT90, HXT4mm, 5.5mm. 200Amp+ capable. Global shipping.

Modified Stealth Fighter - Force air cooled motor @ 6KW, Adaptto Mini-E. 49AH, 52V 18650 - 2.5Kwhr
Cowardlyducks - Stealth Fighter Videos

BikeE recumbent commuter - 9C, 6Fet Grinfineon, internal 17AH, 52V, + on-board solar.

Ebike Garage - My YouTube Ebike ramblings.

User avatar
fechter   100 GW

100 GW
Posts: 13260
Joined: Dec 31 2006 3:23pm
Location: California Bay Area, USA

Re: JP spot welder

Post by fechter » Mar 07 2019 9:01am

You could just use a magnet to see if it's nickel plated steel.
"One test is worth a thousand opinions"

User avatar
Offroader   10 MW

10 MW
Posts: 2300
Joined: Sep 08 2013 9:03pm
Location: USA

Re: JP spot welder

Post by Offroader » Mar 07 2019 8:46pm

fechter wrote:
Mar 07 2019 9:01am
You could just use a magnet to see if it's nickel plated steel.
Nope, 99% nickel is also magnetic so a magnet will tell you nothing.

Instead of salt water use Hydrogen Peroxide , vinegar, and salt and that will really speed up the test to almost instantly start to bubble and corrode. Salt water will rust steel nickel strips but it takes like over 24 hours or so to show anything.

Best is probably just to grind it, yeah you will get a couple of sparks with nickel but nothing like you would with steel.

If that .2 nickel is real I recommend to buy some from the link because it is difficult to find genuine .2 nickel.

.2 nickel is probably as thick as you can go before the weld becomes too weak. .3 nickel is too thick and you will not get good welds.