Spot Welding Copper Strips to 18650 Battery Cells

Batteries, Chargers, and Battery Management Systems.
Post Reply
vex_zg   100 W

100 W
Posts: 178
Joined: Mar 06 2016 6:07pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by vex_zg » Sep 20 2017 6:14am

ridethelightning wrote:
vex_zg wrote:
qwerkus wrote:Anyone tried to weld or solder 5*0.2mm nickel plated copper solar bus wire ? It's cheap, supposedly copper and already protected against corrosion and, with a cross sectional area of 1mm2, it should be able to handle 12A. I wonder how the plating would influence the welding process.
I just ordered, will report in few weeks.
great. im interested to know what happens.
i suspect the tinned coating might sort of explode with welding, as the current will need to be very high to weld the copper.
yeah, tin sort of boils and explodes when you weld. But It's worth a try for couple of $. Zink/nickel plating of copper seems to be easy but I haven't yet had time to explore how this plating impacts welding.

User avatar
ridethelightning   1 MW

1 MW
Posts: 1912
Joined: Jul 21 2013 9:48pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by ridethelightning » Sep 20 2017 6:21am

i did a while ago and was not impressed.
i Ni plated the copper myself, and tried spotwelding it. the results were not too good from memory, but perhaps i was doing it wrong.
they do use it in power tool packs though, with spotwelding so there must logically be a way. it would be a nice material.

geckocycles   1 W

1 W
Posts: 51
Joined: May 05 2013 11:54am
Location: Parker, CO
Contact:

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by geckocycles » Sep 22 2017 10:33am

vex_zg wrote:i tried tungsten, molybdenum, 30-70 copper tungsten. Tested for welding copper, nickel, copper-nickel.

pure copper electrodes still work best for me. Tungsten/molybdenum cause more sparks and blowouts and stick much more.

I have not yet tried zirconium copper (the electrodes I bought are quite big in diameter so need some machining first)

Anybody willing to experiment can get cheap on aliexpress/ebay.

Beware though - machining tungsten and molybden is quite hard. Those are hard materials. Eats grinding stone like it was cake.
Use green grinding wheels, aluminum oxide wheels will dissolve grinding tungsten.

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11825
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by spinningmagnets » Jan 07 2018 9:53pm

https://endless-sphere.com/forums/viewt ... 5#p1349212

" Hummina Shadeeba » Sun Jan 07, 2018 6:30 pm

new info for me is that sodium benzotriazole is a good copper corrosion inhibitor. you can just dip the copper. haven't done it yet. electroplating [nickel] is pretty damn fun though"

xxxxxxxxxxxxxxxxxxx

ES member willow is having success spot welding thin 0.10mm copper

viewtopic.php?f=14&t=68005&sid=f18c217a ... 0#p1348986

Hummina Shadeeba   100 MW

100 MW
Posts: 2537
Joined: Apr 25 2014 10:26pm
Location: sausalito cali..up the hill in front of the cruising club.

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Hummina Shadeeba » Jan 13 2018 4:32am

it looks like the "boss level" welder has no trouble with .1mm copper strip and this guide, which seems more conservative than most, shows .1mm nickel x7mm strip doing 3amps comfortably, so with copper being 4 times as conductive couldn't I do a .1mm x 28MM FOLDED STRIP and that would net me 48 amps?

with the low amount of contact of a spot weld how many welds would be best on each cell



chart from here:
https://endless-sphere.com/forums/viewt ... ding+18650
Attachments
Cu,%20Ni,%20Steel%20efficiency%20chart.png
Cu,%20Ni,%20Steel%20efficiency%20chart.png (43.32 KiB) Viewed 4020 times

vex_zg   100 W

100 W
Posts: 178
Joined: Mar 06 2016 6:07pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by vex_zg » Jan 14 2018 10:45am

.1mm copper is a really thin thing. Yes weldable, some people use it, but it's really weak mechanically. I'd rather use double .2mm nickel for the same conductivity. That's just my opinion, some will disagree.

Hummina Shadeeba   100 MW

100 MW
Posts: 2537
Joined: Apr 25 2014 10:26pm
Location: sausalito cali..up the hill in front of the cruising club.

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Hummina Shadeeba » Jan 19 2018 4:40pm

I have some .14mm copper and it is weak but maybe that's actually a good thing. not saying necessarily and would depend on each instance but if the strip can bend then it isn't putting the strain on the welded connection to the cell

User avatar
Willow   10 kW

10 kW
Posts: 812
Joined: Sep 06 2011 7:42pm
Location: Tasmania

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Willow » Jan 20 2018 8:28pm

vex_zg wrote:
Jan 14 2018 10:45am
.1mm copper is a really thin thing. Yes weldable, some people use it, but it's really weak mechanically. I'd rather use double .2mm nickel for the same conductivity. That's just my opinion, some will disagree.
Like I've said here before... the cells should be held together with glue or in holders. Never rely on the electrical connections to hold the batteries together... nickel, copper or otherwise, the spot welds are simply not enough... and hence they should bare no mechanical loading.

fourbanger   100 W

100 W
Posts: 205
Joined: Jul 17 2014 10:09pm
Location: Victoria B.C. Canada

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by fourbanger » Jan 22 2018 1:14am

So, these exist:

https://www.aliexpress.com/store/produc ... 407dNQrXvq

https://www.aliexpress.com/store/produc ... f54fsgLTdK

Don't find them much inspiring, myself, and a bit rich for my blood. Just thought I'd offer it up as an option (of sorts).

Hummina Shadeeba   100 MW

100 MW
Posts: 2537
Joined: Apr 25 2014 10:26pm
Location: sausalito cali..up the hill in front of the cruising club.

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Hummina Shadeeba » Feb 14 2018 10:30pm

this one is most versatile I've see and only 2 cells. really nice design. easy to print.


https://www.aliexpress.com/item/High-Qu ... autifyAB=0


is there a reason not to do a single strip of .13mm strip 30mm wide and fold it in half? I read doing copper on copper is hard and rather just do this and keep within the niobi guidelines. a hair away from welding the pack and wondering why i dont read of more people doing thin copper and folding.

Joachim   1 kW

1 kW
Posts: 435
Joined: Jul 30 2015 1:02pm
Contact:

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Joachim » Feb 22 2018 3:36pm

i have seen a compleet e-bike pack welded 2.5mm nickel platet copper so there are companys use copper for the battery packs.
This is a Taiwan company.

I will shoot pics of a pack and post here.

The welds are not so strong like nickel..but oke.you can see they use more current to get good welds an also a cut in the strips for maximal strong welds/good current flow over the tops from the cells.

E1Allen   1 mW

1 mW
Posts: 19
Joined: Mar 26 2018 4:20am

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by E1Allen » Apr 13 2018 12:54am

So. If I have .2mm copper strips with the nickel tabs spot welded to it. Could I take a 30mm wide copper strip and fold it to 10mm wide to increase the overall area and amp carrying ability while keeping it less than 18650 width. In the future I'm looking to do a 30q pack in the 8p size or more. But that puts you above 160a. Granted it's not a continuous draw number. I'm wondering how well some of the large P copper welded packs you guys have made are holding up and what kind of amp draw you're able to pull.

Philaphlous   1 kW

1 kW
Posts: 431
Joined: Mar 28 2017 7:17am

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Philaphlous » Apr 13 2018 5:01am

Hummina Shadeeba wrote:
Jan 13 2018 4:32am
it looks like the "boss level" welder has no trouble with .1mm copper strip and this guide, which seems more conservative than most, shows .1mm nickel x7mm strip doing 3amps comfortably, so with copper being 4 times as conductive couldn't I do a .1mm x 28MM FOLDED STRIP and that would net me 48 amps?

with the low amount of contact of a spot weld how many welds would be best on each cell



chart from here:
https://endless-sphere.com/forums/viewt ... ding+18650
Thanks for the chart! Good to know my 3.5mm pure copper wick wire is going to deliver a ton of amps without any issues!

User avatar
ridethelightning   1 MW

1 MW
Posts: 1912
Joined: Jul 21 2013 9:48pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by ridethelightning » Apr 13 2018 7:18am

E1Allen wrote:
Apr 13 2018 12:54am
So. If I have .2mm copper strips with the nickel tabs spot welded to it. Could I take a 30mm wide copper strip and fold it to 10mm wide to increase the overall area and amp carrying ability while keeping it less than 18650 width. In the future I'm looking to do a 30q pack in the 8p size or more. But that puts you above 160a. Granted it's not a continuous draw number. I'm wondering how well some of the large P copper welded packs you guys have made are holding up and what kind of amp draw you're able to pull.
160 A from 8p30Q is a bit ambitious.
it might do it for a second but the sag will make it not very fun and you will be trashing the cells.

12p is another matter :D

my copper packs, 22s 12p and 18p 30q are holding up nicely.

User avatar
ridethelightning   1 MW

1 MW
Posts: 1912
Joined: Jul 21 2013 9:48pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by ridethelightning » Apr 14 2018 6:46am

just thought id put it out there-

has anyone toyed with using multiple mots in parallel to get enough juice to do copper welding?

perhaps someone could shed some light on weather or not it would, in theory, work and any other hints that would help?

cheers.

User avatar
Matador   100 kW

100 kW
Posts: 1042
Joined: Jun 29 2016 10:00pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Matador » May 20 2018 2:25pm

Any progress on this topic? I got myself a 0.005" (0.127mm) roll of 110 aka C11000 copper (IACS 101%), 12 feet by 12 inch.
16.99$ from K&S precision metal (Item stock number : #6020).

I always had hopes to do something laike that:
PICT0097.JPG
PICT0097.JPG (92.23 KiB) Viewed 3344 times
ref: viewtopic.php?f=14&t=68005&start=100#p1134835
copper.jpg
copper.jpg (224.29 KiB) Viewed 3344 times
ref: viewtopic.php?f=14&t=68005&start=650#p1348986

litespeed   100 kW

100 kW
Posts: 1440
Joined: Aug 11 2010 4:42pm
Location: O’Fallon, Missouri

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by litespeed » May 21 2018 4:34pm

So did you buy directly from them? Looks like it could work?

Tom
I'm married so you know I'm no stranger to pain!

User avatar
Matador   100 kW

100 kW
Posts: 1042
Joined: Jun 29 2016 10:00pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Matador » May 21 2018 5:56pm

No I bought in an art store in NYC in chinatown on Lafayette st, cant temember the name

User avatar
Willow   10 kW

10 kW
Posts: 812
Joined: Sep 06 2011 7:42pm
Location: Tasmania

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Willow » May 22 2018 4:27pm

If you are using copper it of utmost importance to never touch it with bare skin and to clean it thoroughly with isopropal alcohol before spotwelding. Avoid corrosion - oils and acids in the skin are not what you want on the copper, especially when there is current flowing through it. If it has been touched/fingerprinted - don't use these bits.

kdog   10 kW

10 kW
Posts: 694
Joined: Feb 02 2014 9:22pm
Location: hobart, tasmania

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by kdog » May 25 2018 6:05am

Hey RTL
You can parallel transformers, it's pretty simple but you have to get the windings around the right way otherwise you are shorting one to the another.
Attachments
images.jpeg
images.jpeg (25.38 KiB) Viewed 3240 times

User avatar
Willow   10 kW

10 kW
Posts: 812
Joined: Sep 06 2011 7:42pm
Location: Tasmania

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by Willow » May 26 2018 3:42am

that would be spectacular!

User avatar
ridethelightning   1 MW

1 MW
Posts: 1912
Joined: Jul 21 2013 9:48pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by ridethelightning » May 26 2018 8:00am

kdog wrote:
May 25 2018 6:05am
Hey RTL
You can parallel transformers, it's pretty simple but you have to get the windings around the right way otherwise you are shorting one to the another.
thx for that.
i keep seeing ovens around but like in a dream, its never the time to get them :|
when i get them together, (i think ill try 3 or 4) should be fun times.

another thing, the arc welder spotwelder i have actually has 2 primaries and 2 secondaries.
so far i have only been using it with one primary engaged i think, as the 2 primaries in series gave too low voltage at output so we just left one disconnected, which was ok for nickel, but perhaps putting the 2 primaries in parallele might be the key here..

and perhaps ditching the central dampening block alogether.

garolittle   1 kW

1 kW
Posts: 442
Joined: Mar 03 2018 1:06pm
Location: Augusta, GA U.S.A
Contact:

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by garolittle » Jun 24 2018 7:38pm

spinningmagnets wrote:
Jun 26 2017 7:22pm
Here is a recent high-amp cordless tool battery pack. The busses are verified to be copper (with a nickel-plate for corrosion and to help make spot-welding easier). Notice how much longer the slot is, compared to the more common pure nickel strips in the past...

Image

I have not finished reading all of these posts but is there any way to purchase the nickel-plated copper busses depicted in the picture? This seems like an ideal solution. Thanks for an awesome forum. Gary

greenno   100 µW

100 µW
Posts: 8
Joined: Sep 26 2018 2:44pm

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by greenno » Oct 22 2018 6:54pm

Just found this thread and loved it. Got a lot of good info. Started making my own batteries after buying and building up a BBSHD kit for my own bike and was using a typical shark pack 13.5ahs. After numerous rides I found I wanted more capacity for riding longer distances. So I did a little research and purchased a Sunko 709A spot welder and .15 x 8mm nickel strips. Designed a 31.5ah battery to fit inside the main triangle of my bike complete with BMS packed into a triangle zip bag with some padding around it and it fits good. After numerous rides I needed to open up pack as it wasn't performing like it should and found a number of spot welds had come loose from vibration but it was typically only on the top layer of strips the original bottom layers were good.
So I was wondering why you couldn't just use solid nickel sheet as a solid piece instead of using copper and spot welding a nickel strip across the hole to weld onto the battery surface? I get that using copper increases current capacity as far as series connections go but with the motor controller limiting 30a max with the extra surface area from the solid nickel piece you would be fine. Found a place on line that sells 201 pure nickel 6"x12"x.005" for $6.95 each. I tried the .010 thick piece but this welder doesn't have enough power for a good penetrating weld onto a battery. We'll see if the thinner piece works or not. Any ideas? Im all ears.

User avatar
spinningmagnets   100 GW

100 GW
Posts: 11825
Joined: Dec 21 2007 10:27pm
Location: Ft Riley, NE Kansas

Re: Spot Welding Copper Strips to 18650 Battery Cells

Post by spinningmagnets » Oct 22 2018 7:03pm

The design that I am currently impressed by is a broad sheet of copper as a bus-plate, with round holes over the cell locations. The connection between the copper bus-plates and the cell could initially be nickel, and depending on how experiments progress, possibly nickel-plated copper..

Post Reply