Post by thunderheart » May 21 2019 12:14am

Samsung INR18650-30Q is a high capacity 3000mAh Li-ion cell of 18650 size which supports continuous discharge at up to 15A. It's can be called a high drain cell or even a mid-to-high drain one.
Image

The battery was bought from my reliable supplier (Queen Battery) and tested with ZKETECH EBC-A20 and a self-made battery holder. It's a PC-connected battery tester supporting 4-wire measuring and discharging at up to 20A.
Image

I've used version 3.0 of my battery holder based on 0.5mm thick pure copper terminals
Image
Image

I've followed all the prescriptions of the IEC61960-2003 standard concerning battery's capacity measurement. Before each discharging cycle each battery was charged at standard charge current mentioned in its datasheet to charge end voltage. Before each discharging or charging i've held a 1-1.5hrs pause. The environment temperature was 23.0-24.5°C. To be sure in results i've done each test minimum twice (usually 3-4 times).


Samsung INR18650-30Q

My cell has the following marking: INR18650-30Q SAMSUNG SDI 136.
Image

The main specs from Samsung 30Q datasheet:
Nominal capacity: 3000mAh
Nominal voltage: 3.6V
Standard charge current: 1.5A / 150mA cut-off
Maximum charge current: 4A / 100mA cut-off
Charge end voltage: 4.20V
Max. continuous discharge current: 15A (5C)
Discharge cut-off voltage: 2.5V
AC impedance at 1KHz: ≤26mΩ
Max weight: 48g

Measured initial DC IR at 3A in fully charged condition was 16.0±0.7mΩ (measured using EB Tester Software's tool)

Measured weight of the tested cell was 45.6g
Image

Samsung 30Q capacity test results:
Image
At 0.2C (0.6A) 30Q's capacity appeared to be a bit higher than 3100mAh vs 3000mAh declared - a nice start but no surprise. All the way up to 15A it remains above 2900mAh and the curves look excellent. 2.5V discharge cut-off is another advantage which allows to use a wider voltage range. 30Q is a good high drain cell which is a high capacity one at the same time - that's why it's so popular.

Here is the video version of this review:
Image


Check out my YouTube channel for batteries, chargers and other stuff reviews.
I've launched my blog where you can find all my reviews in one place. Every new test/review will be first published on YouTube and in the blog. I'll be happy to see new subscribers, comments, suggestions and just your thoughts.
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » May 21 2019 7:39am

stellar effort as usual and fine result

User avatar
izeman   100 GW

100 GW
Posts: 5048
Joined: Jun 21 2011 8:25am
Location: Vienna, Austria
Contact:

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by izeman » May 21 2019 10:39am

Thanks for the test. I have good results with this cell as well using it in a 15s10p pack at 60A maximum discharge (so no big stress).
Are you planing to do a cycle number test as well? Capacity after 100, 500 or 1000 charges?

litespeed   100 kW

100 kW
Posts: 1404
Joined: Aug 11 2010 4:42pm
Location: St. Peters, Missouri

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by litespeed » May 21 2019 8:45pm

I built a 20s15p with these cells and even pulling 200 amps (very seldom but sometimes!😬) with my MaxE the voltage stays so high.......crazy powerful.

Huge change from the 20s15p VTC3 pack I built some time back.

Love them.

Tom
I'm married so you know I'm no stranger to pain!

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by thunderheart » Jun 02 2019 10:03am

izeman wrote:
May 21 2019 10:39am
Thanks for the test. I have good results with this cell as well using it in a 15s10p pack at 60A maximum discharge (so no big stress).
Are you planing to do a cycle number test as well? Capacity after 100, 500 or 1000 charges?
Thanks izeman!
No, i'm not doing cycle life tests
litespeed wrote:
May 21 2019 8:45pm
Love them.
Hi Tom!
Lot of people love them)) They're worth it))
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

User avatar
Drunkskunk   100 GW

100 GW
Posts: 7167
Joined: Apr 14 2007 11:37am
Location: Dallas, Texas. U.S.A.

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by Drunkskunk » Jun 03 2019 4:23pm

Awesome. I've been looking at these cells for an upcoming project. Looks great!
Buy the ticket, take the ride.
Monster Bike:http://endless-sphere.com/forums/viewto ... =6&t=38667

drbenjamin   1 mW

1 mW
Posts: 17
Joined: Jun 17 2014 2:22pm
Location: Redmond, WA USA

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by drbenjamin » Jun 04 2019 1:24pm

So does a 2.5V discharge cutoff mean that a 14S pack can be used down to 39.8V and still be at 20%?

(4.2-2.5 = 1.7V/cell total capacity, 0.34V = 20% capacity. 2.5V x 14 = 35V at cutoff, .34x14 = 4.*V for 20% residual capacity)

Asking because 42V seems to be a default LVC for 14S and that would be 30% by my calcs

Thanks!

User avatar
izeman   100 GW

100 GW
Posts: 5048
Joined: Jun 21 2011 8:25am
Location: Vienna, Austria
Contact:

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by izeman » Jun 04 2019 2:32pm

drbenjamin wrote:
Jun 04 2019 1:24pm
So does a 2.5V discharge cutoff mean that a 14S pack can be used down to 39.8V and still be at 20%?

(4.2-2.5 = 1.7V/cell total capacity, 0.34V = 20% capacity. 2.5V x 14 = 35V at cutoff, .34x14 = 4.*V for 20% residual capacity)

Asking because 42V seems to be a default LVC for 14S and that would be 30% by my calcs
If you look at the discharge curve you'll notive that it is NOT LINEAR, and it differs dependent on discharge current. So you need to take your discharge current, choose the appropriate curve and check where it is for 20% or 600mA left. This is under load though. If you take the lowest discharge curve (purple) it says that at 3.3V (with very little load - so almost resting state) it has 20% capacity left = 46.2V for 14s. At 2.8V=39.8V it's EMPTY.

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 04 2019 4:44pm

In practice even 3.1Vpc is empty, insignificant range left after that

And you're killing longevity even going that low.

Depending on C-rate of course, as a bounceback resting V that's pretty mainstream

User avatar
izeman   100 GW

100 GW
Posts: 5048
Joined: Jun 21 2011 8:25am
Location: Vienna, Austria
Contact:

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by izeman » Jun 05 2019 12:15am

john61ct wrote:
Jun 04 2019 4:44pm
In practice even 3.1Vpc is empty, insignificant range left after that
Normally I'd say correct, but this cell has a lower discharge cut off then other cells. Where you normally got till 3.0V max, this cells goes to 2.8V. But of course this is not where the meat is anymore. 8)

User avatar
ridethelightning   1 MW

1 MW
Posts: 1869
Joined: Jul 21 2013 9:48pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by ridethelightning » Jun 05 2019 1:37am

subscribe

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 05 2019 5:29am

izeman wrote:
john61ct wrote:
Jun 04 2019 4:44pm
In practice even 3.1Vpc is empty, insignificant range left after that
Normally I'd say correct, but this cell has a lower discharge cut off then other cells. Where you normally got till 3.0V max, this cells goes to 2.8V. But of course this is not where the meat is anymore. 8)
Going anywhere near that low regularly will murder cycle lifetime.

And again, really not significantly greater range

User avatar
teslanv   100 MW

100 MW
Posts: 2675
Joined: Nov 03 2013 8:42pm
Location: Bellevue, WA - USA
Contact:

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by teslanv » Jun 05 2019 8:46am

I've been specifying the Samsung 30Q cells for my pack builds for the last 2 years. They are good enough that I haven't had the urge to experiment with any other cells.
So yeah, they get my vote. :bigthumb:
DD Hubs, Batteries, Controllers & Custom Ebikes.
http://westcoastelectrics.com
West Coast Electric Cycles
Bellevue, WA
USA

User avatar
ridethelightning   1 MW

1 MW
Posts: 1869
Joined: Jul 21 2013 9:48pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by ridethelightning » Jun 05 2019 9:25am

I have built 4 large packs with these. they are ok if you have plenty in parallel.
after all the initial discussion about them being good chemistry, like the 20R and 25R cells, I was not very happty to see that they can lose capacity very fast compared to other cells, and my not be that good with regard to cycle life, especially if used as their specs indicate, 15A discharge etc.

larsb   1 MW

1 MW
Posts: 1640
Joined: Dec 10 2014 5:12am
Location: Gothenburg, Sweden

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by larsb » Jun 05 2019 9:36am

Edit: incorrect data removed
Last edited by larsb on Jun 06 2019 5:07am, edited 3 times in total.
Ride on!

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 05 2019 10:05am

Just from a quick skim, there are so many wildly inaccurate claims on one page I would discount anything written by that author.

And Battery University the site that they're disputing, also has plenty of misinformation, certainly over-generalizations, so would be skeptical of anyone taking it that seriously

larsb   1 MW

1 MW
Posts: 1640
Joined: Dec 10 2014 5:12am
Location: Gothenburg, Sweden

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by larsb » Jun 05 2019 10:56am

Edit: incorrect data removed
Last edited by larsb on Jun 06 2019 5:05am, edited 1 time in total.
Ride on!

drbenjamin   1 mW

1 mW
Posts: 17
Joined: Jun 17 2014 2:22pm
Location: Redmond, WA USA

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by drbenjamin » Jun 05 2019 3:03pm

izeman wrote:
Jun 04 2019 2:32pm


If you look at the discharge curve you'll notive that it is NOT LINEAR, and it differs dependent on discharge current. So you need to take your discharge current, choose the appropriate curve and check where it is for 20% or 600mA left. This is under load though. If you take the lowest discharge curve (purple) it says that at 3.3V (with very little load - so almost resting state) it has 20% capacity left = 46.2V for 14s. At 2.8V=39.8V it's EMPTY.
Thanks for the explanation, it makes sense now that you point out that amps (not volts) is the capacity we are interested in.

Thanks again!
Last edited by drbenjamin on Jun 05 2019 5:34pm, edited 1 time in total.

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 05 2019 3:31pm

I have never seen any rechargeable battery chemistry where the curve between average DoD and lifetime cycles did not have a **very** strong causative slope, and all in the same direction.

Claims of such an extraordinary exception would carry the burden of proof, I'm certainly not going to bother building a case for something I consider as obvious as "cells wired in parallel tend toward the same voltage".

MesquiteTim   10 µW

10 µW
Posts: 6
Joined: May 30 2019 4:42pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by MesquiteTim » Jun 05 2019 8:38pm

How would you rate this cell against the 40T?

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 05 2019 10:16pm


drbenjamin wrote:you point out that amps (not volts) is the capacity we are interested in.
Capacity is mAh / Ah / Wh

amps (just like watts) is an instantaneous measure of flow rate, not quantity of energy.

So 20% of the capacity remaining at 3.3V loaded is not "600mA left" but 600mAh.

units are important


User avatar
izeman   100 GW

100 GW
Posts: 5048
Joined: Jun 21 2011 8:25am
Location: Vienna, Austria
Contact:

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by izeman » Jun 11 2019 3:09am

john61ct wrote:
Jun 05 2019 10:16pm
So 20% of the capacity remaining at 3.3V loaded is not "600mA left" but 600mAh.
Damnit. Such a mistake happening to me... Me, that constantly corrects other people's posts about SE units, and urges them to use the correct one.
Shame on me! Of course it's mAh.

john61ct   1.21 GW

1.21 GW
Posts: 3730
Joined: Dec 18 2018 2:06pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by john61ct » Jun 11 2019 9:33am

Oh the shame 8-)

User avatar
thunderheart   100 W

100 W
Posts: 212
Joined: Oct 08 2017 10:01am
Location: Armenia

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by thunderheart » Jun 13 2019 1:30am

ridethelightning wrote:
Jun 05 2019 9:25am
I was not very happty to see that they can lose capacity very fast compared to other cells, and my not be that good with regard to cycle life, especially if used as their specs indicate, 15A discharge etc.
At 15A discharge the manufacturer guarantees 60% of the initial capacity at 250th cycle so nobody promised some great cycle life at max discharge rate.
MesquiteTim wrote:
Jun 05 2019 8:38pm
How would you rate this cell against the 40T?
Hmmm... Are you serious?)))) 40T is a 21700 cell, by the way
Yinlong LTO Lithium Titanate safety tests: https://youtu.be/eAUYbSDEy6I
Toshiba SCiB LTO Lithium Titanate safety tests:https://youtu.be/XsrRDZxEFQE

LG M50 vs Samsung 48G:https://youtu.be/KGJDogOG4zw
LiFePO4: QB26650 2500mAh 50A vs A123 ANR26650M1B: https://youtu.be/GOSkte11lRc

User avatar
ridethelightning   1 MW

1 MW
Posts: 1869
Joined: Jul 21 2013 9:48pm

Re: Samsung 30Q - high drain 18650 Li-ion cell's capacity test

Post by ridethelightning » Jun 13 2019 6:34am

thunderheart wrote:
Jun 13 2019 1:30am
At 15A discharge the manufacturer guarantees 60% of the initial capacity at 250th cycle so nobody promised some great cycle life at max discharge rate.
the max claimed peak power for this cell is like 20A or 25A something(sorry cant remember exactly)
so 60% initial capacity at 250 cyles at only 15 A., which i thought they could do comfortably...
not impressed.
so really this is not really a high capacity/high discharge cell at all if you want a decent lifespan.