I'll start with my general observation first. I have some A123 20Ah pouch cells lying around. These were 'quality cells' (bought not from VictPower), measured exactly 20.0Ah. Due to long storage and some test equipment being hooked up, some of them got self-discharged (down to 0.2V) over the time and puffed badly.
So I decided to make a test with them. Charged at 0.5C rate fully. ~18Ah went in (notice a drop from previous 20Ah). And left them to rest for a month.
And guess what. A month passed and all puffed cells are no longed puffed. Swelling reduced to almost original state. Capacity dropped to 18Ah, permanently. The victims still have some wrinkles as a proof of previous puffing. Also their Ri increased from ~0.9mΩ to 2-3 mΩ.
Now, here's my theory: VictPower sells crappy cells, that they get for scrap metal price. Usually these cells are puffed, so they pre-charge them a bit and ship out. Many of their cells have wrinkles or mechanical damage, as well as very different tabs: ones have perforation (fuse), others don't, some have badly cut perforation and some of cell's foil cut-off, some have unevenly cut-off tabs, that are a dead giveaway they were removed from a pack.
Received a pallet of cells from client, who bought them from VictPower.
So, all of you measuring "18Ah" capacity... You get what you pay for. Junk.
So I decided to make a test with them. Charged at 0.5C rate fully. ~18Ah went in (notice a drop from previous 20Ah). And left them to rest for a month.
And guess what. A month passed and all puffed cells are no longed puffed. Swelling reduced to almost original state. Capacity dropped to 18Ah, permanently. The victims still have some wrinkles as a proof of previous puffing. Also their Ri increased from ~0.9mΩ to 2-3 mΩ.
Now, here's my theory: VictPower sells crappy cells, that they get for scrap metal price. Usually these cells are puffed, so they pre-charge them a bit and ship out. Many of their cells have wrinkles or mechanical damage, as well as very different tabs: ones have perforation (fuse), others don't, some have badly cut perforation and some of cell's foil cut-off, some have unevenly cut-off tabs, that are a dead giveaway they were removed from a pack.
Received a pallet of cells from client, who bought them from VictPower.
So, all of you measuring "18Ah" capacity... You get what you pay for. Junk.