Recently, I got a 12V 95AH VRLA/AGM lead acid battery with just 11.17V. I found it is dry inside. I treated it as a regular lead acid battery. I filled it up with distilled water and charged it with a variable power supply. I set the current to 4A and charge it for about 6 hours. The voltage went up to 12.51V. But after sitting over night, the voltage dropped down to 11.97V. Also, during charging, I found just only one cell was bubbling. Will that mean something wrong? Should I try charging it with higher current (or 4A is good enough but just takes longer time)?

I have checked the internet, they just suggest to charge AGM battery with the special AGM battery charger. Could somebody please give me some detailed information on how to properly charge an AGM battery with just regulated power supplies? I have a 0-60V, 0-5A power supply and a 13.8V, 23A power supply. I also have a 1A trickle car charger.








Reply
 

Attachments

  • Mercedes 12V battery label.jpeg
    Mercedes 12V battery label.jpeg
    563.5 KB · Views: 0
Last edited:
None of the cells should bubble in normal charging or operation. It's fairly likely the battery is damaged from whatever event dried it out (extended floating charging above voltage or current limits is most common), See the

OVERCHARGING A LEAD ACID BATTERY​

section in PowerSonic's lead-acid charging page (quoted below)

HOW TO CHARGE A LEAD ACID BATTERY​

Dependable performance and long service life of your sealed lead acid battery will depend upon correct battery charging. Following incorrect charging procedures or using inadequate charging equipment can result in decreased battery life and/or poor battery performance. The selection of a suitable SLA battery charger and the methods used to charge it is just as important as choosing the right battery for the application.
Power Sonic recommends you select a charger designed for the chemistry of your battery. This means we recommend using a sealed lead acid battery charger, like the the A-C series of SLA chargers from Power Sonic, when charging a sealed lead acid battery.

BATTERY CHARGING TECHNIQUES​

Sealed lead acid batteries may be charged by using any of the following charging techniques:
  • Constant Voltage
  • Constant Current
  • Taper Current
  • Two Step Constant Voltage
To obtain maximum battery service life and capacity, along with acceptable recharge time and economy, constant voltage-current limited charging is best.
To charge a sealed lead acid battery, a DC voltage between 2.30 volts per cell (float) and 2.45 volts per cell (fast) is applied to the terminals of the battery. Depending on the state of charge (SoC), the cell may temporarily be lower after discharge than the applied voltage. After some time, however, it should level off.
During charge, the lead sulfate of the positive plate becomes lead dioxide. As the battery reaches full charge, the positive plate begins generating dioxide causing a sudden rise in voltage due to decreasing internal resistance. A constant voltage charge, therefore, allows detection of this voltage increase and thus control of the current charge amount.

BATTERY CHARGING CHARACTERISTICS​

During constant voltage or taper charging, the battery’s current acceptance decreases as voltage and state of charge increase. The battery is fully charged once the current stabilizes at a low level for a few hours. There are two criteria for determining when a battery is fully charged: (1) the final current level and (2) the peak charging voltage while this current flows.
1683583670248.png
Typical sealed lead acid battery charge characteristics for cycle service where charging is non-continuous and peak voltage can be higher.
1683583678920.png
Typical characteristics for standby service type battery charge. Here, charging is continuous and the peak charge voltage must be lower.

BATTERY CHARGING METHODS​

Selecting the appropriate charging method for your sealed lead acid battery depends on the intended use (cyclic or float service), economic considerations, recharge time, anticipated frequency and depth of discharge (DoD), and expected service life. The goal of any charging method is to control the charge current at the end of the charge.

CONSTANT VOLTAGE CHARGING​

Constant voltage charging is the best method to charge sealed lead acid batteries. Depending on the application, batteries may be charged either on a continuous or non-continuous basis. In applications where standby power is required to operate, for example a security system or uninterruptible power supply (UPS), when the AC power has been interrupted, continuous float charging is recommended. Non-continuous cyclic charging is used primarily with portable equipment where charging on an intermittent basis is appropriate, such as electric wheelchairs and mobile medical carts.
The constant voltage charge method applies a constant voltage to the battery and limits the initial charge current. It is necessary to set the charge voltage according to specified charge and temperature characteristics. Inaccurate voltage settings can cause either over-charge or under-charge. This charging method can be used for both cyclic and standby applications.
1683583645170.png
Constant voltage charging circuit
1683583653988.png
Constant voltage charging characteristics

CONSTANT CURRENT CHARGING​

Constant current charging is suited for applications where discharged ampere-hours of the preceding discharge cycle are known. Charge time and charge quantity can easily be calculated, however an expensive circuit is necessary to obtain a highly accurate constant current. Monitoring of charge voltage or limiting of charge time is necessary to avoid excessive overcharge of the battery.
While this charging method is very effective for recovering the capacity of a SLA battery that has been stored for an extended period of time, or for occasional overcharging to equalize cell capacities, it lacks specific properties required in today’s electronic environment.

TAPER CURRENT CHARGING​

The taper current charging method is not recommended as it is somewhat abusive of sealed lead acid batteries and can shorten service life. However, because of the simplicity of the circuit and low cost, taper current charging is extensively used to charge multiple numbers and/or for cyclic charging.
When using a taper current battery charger the charger time should be limited or a charging cut-off circuit needs to be incorporated to prevent over-charge.
In a taper current charging circuit, the current decreases in proportion to the voltage rise. When designing a taper charger always consider power voltage fluctuations. In this event the internal resistance drop will convert to heat. Heat generated by the circuit should be measured and if required a heat sink should be incorporated in the design.1683583585366.png
Taper current charging circuit
1683583624159.png
Taper current charging characteristics for this type of basically unregulated charger

OVERCHARGING A LEAD ACID BATTERY​

As a result of too high a charge voltage excessive current will flow into the battery, after reaching full charge, causing decomposition of water in the electrolyte and premature aging.
At high rates of overcharge a battery will progressively heat up. As it gets hotter, it will accept more current, heating up even further. This is called thermal runaway and it can destroy a battery in as little as a few hours.

UNDERCHARGING A LEAD ACID BATTERY​

If too low a charge voltage is applied, the current flow will essentially stop before the battery is fully charged. This allows some of the lead sulfate to remain on the electrodes, which will eventually reduce battery capacity.
Batteries which are stored in a discharged state, or left on the shelf for too long, may initially appear to be “open circuited” or will accept far less current than normal. This is caused by a phenomenon called “sulfation”. When this occurs, leave the charger connected to the battery. Usually, the battery will start to accept increasing amounts of current until a normal current level is reached. If there is no response, even to charge voltages above recommended levels, the battery may have been in a discharged state for too long to recover, and in which case a replacement SLA battery will be needed.

LEAD ACID BATTERY CYCLE CHARGING​

Cyclic (or cycling) applications generally require recharging be done in a relatively short time. The initial charge current, however, must not exceed 0.30 x C amps. Just as battery voltage drops during discharge, it slowly rises during charge. Full charge is determined by voltage and inflowing current. When, at a charge voltage of 2.45 ± 0.05 volts/cell, the current accepted by the battery drops to less than 0.01 x C amps (1% of rated capacity), the battery is fully charged and the charger should be disconnected or switched to a float voltage of 2.25 to 2.30 volts/cell. The voltage should not be allowed to rise above 2.45 ± 0.05 volts/cell.

LEAD ACID BATTERY STANDBY CHARGING​

Standby applications generally do not require that the battery be charged as fast or as frequently as in cycle operation. However, the battery must be kept constantly charged to replace the energy that is expended due to internal loss and deterioration of the battery itself. Although these losses are very low in Power Sonic lead acid batteries, they must be replaced at the rate the battery self discharges; at the same time the battery must not be given more than these losses or it will be overcharged. To accomplish this, a constant voltage method of charging called standby or float charging is used.
The recommended constant float voltage is 2.25 – 2.30 volts per cell. Maintaining this float voltage will allow the battery to define its own current level and remain fully charged without having to disconnect the charger from the battery. The trickle current for a fully charged battery floating at the recommended charge voltage will typically hover around the 0.001C rate (7mA for a 7AH battery, for example.)
The float charger is basically a constant voltage power supply. As with cycle chargers, care must be taken not to exceed the initial charge current of 0.30 x C amperes.

TWO STEP CONSTANT VOLTAGE CHARGING​

This method uses two constant voltage devices. In the initial charge phase the high voltage setting is used. When charging is nearly complete and the charge voltage has risen to a specified value (with the charge current decreased), the charger switches the voltage to the lower setting. This method allows rapid charging in cycle or float service without the possibility of overcharging, even after extended charging periods.
1683583721583.png
Dual stage current limited SLA battery charger
1683583730318.png
Two-step constant voltage charging characteristics.

CHARGING 2 OR MORE BATTERIES IN SERIES​

Lead acid batteries are strings of 2 volt cells connected in series, commonly 2, 3, 4 or 6 cells per battery. Strings of lead acid batteries, up to 48 volts and higher, may be charged in series safely and efficiently. However, as the number of batteries in series increases, so does the possibility of slight differences in capacity. These differences can result from age, storage history, temperature variations or abuse.
Fully charged batteries should never be mixed with discharged batteries when charging batteries in series. The discharged batteries should be charged before connection.
When a single constant voltage charger is connected across an entire high voltage string, the same current flows through all cells in the string. Depending on the characteristics of the individual batteries, some may overcharge while others remain in a slightly undercharged condition.
To minimize the effects of individual battery differences, use batteries of the same age, manufacturer, amp hour, and history and, if possible, charge in strings of no greater than 24 or 48 volts.

CHARGING BATTERIES IN PARALLEL​

Lead acid batteries may be used in parallel with one or more batteries of equal voltage. When connecting batteries in parallel, the current from a charger will tend to divide almost equally between the batteries. No special matching of batteries is required. If the batteries of unequal capacity are connected in parallel, the current will tend to divide between the batteries in the ratio of capacities (actually, internal resistances).
When charging batteries in parallel, where different ratios of charge are to be expected, it is best to make provisions to assure that the currents will not vary too much between batteries.

BATTERY TEMPERATURE COMPENSATION​

Power Sonic sealed lead acid batteries perform well both at low and high temperatures. At low temperatures, however, charge efficiency is reduced; at temperatures above 45°C (113°F), charge efficiency increases so rapidly that there is a danger of thermal runaway if temperature compensation is not precise.
The effect of temperature on charge voltage is less critical in float applications than in cyclic use, where relatively high charge currents are applied for the purpose of short recharge times.
Temperature effects should definitely be considered when designing or selecting a charging system. Temperature compensation is desirable in the charging circuit, especially when operating outside the range of 5°C to 35°C
(41°F to 95°F). The temperature coefficient is -2mV/cell/ºC below 20°C (68°F) in float use and -6mV/cell/ ºC below 20°C in cyclic use. For higher temperatures the charge voltage should be correspondingly decreased.
The battery temperature compensation chart below shows the recommended charge voltages for different temperatures based on ambient charge voltage per cell.
TemperatureCyclic Use (V)Float Use (V)
-40°C (-40°F)2.85 – 2.952.38 – 2.43
-20°C (-4°F)2.67 – 2.772.34 – 2.39
-10°C (14°F)2.61 – 2.712.32 – 2.37
0°C (32°F)2.55 – 2.652.30 – 2.35
10°C (50°F)2.49 – 2.592.28 – 2.33
20°C (68°F)2.43 – 2.532.26 – 2.31
25°C (77°F)2.40 – 2.502.25 – 2.30
30°C (86°F)2.37 – 2.472.24 – 2.29
40°C (104°F)2.31 – 2.412.22 – 2.27
50°C (122°F)2.25 – 2.352.20 – 2.25

TOP UP CHARGING SLA BATTERIES​

All batteries lose capacity through self-discharge, it is recommended that a “top up charge” be applied to any battery that has been stored for a long period of time, prior to putting the battery into service.
To successfully top up charge a battery stored for more than 12 months, the open circuit voltage must be higher than 2.0 volts per cell, in this case, always confirm open circuit voltage prior to attempting top up charging.

BATTERY CHARGING EFFICIENCY​

The charging efficiency (η) of a battery is expressed by the following formula:1683583756061.png
The charging efficiency varies depending upon the state of charge of the battery, temperatures, and charging rates. The below graph illustrates the concept of the state of charge and charging efficiency.
The below graph shows Power Sonic sealed lead acid batteries exhibit very high charging efficiency, even when charged at low charging rates.
1683583769372.png
It is always important to match your charger to deliver the correct current and voltage for the battery you are charging. For example, you wouldn’t use a 24V charger to charge a 12V battery.


 
None of the cells should bubble in normal charging or operation. It's fairly likely the battery is damaged from whatever event dried it out (extended floating charging above voltage or current limits is most common), See the

OVERCHARGING A LEAD ACID BATTERY​

section in PowerSonic's lead-acid charging page (quoted below)

HOW TO CHARGE A LEAD ACID BATTERY​

Dependable performance and long service life of your sealed lead acid battery will depend upon correct battery charging. Following incorrect charging procedures or using inadequate charging equipment can result in decreased battery life and/or poor battery performance. The selection of a suitable SLA battery charger and the methods used to charge it is just as important as choosing the right battery for the application.
Power Sonic recommends you select a charger designed for the chemistry of your battery. This means we recommend using a sealed lead acid battery charger, like the the A-C series of SLA chargers from Power Sonic, when charging a sealed lead acid battery.

BATTERY CHARGING TECHNIQUES​

Sealed lead acid batteries may be charged by using any of the following charging techniques:
  • Constant Voltage
  • Constant Current
  • Taper Current
  • Two Step Constant Voltage
To obtain maximum battery service life and capacity, along with acceptable recharge time and economy, constant voltage-current limited charging is best.
To charge a sealed lead acid battery, a DC voltage between 2.30 volts per cell (float) and 2.45 volts per cell (fast) is applied to the terminals of the battery. Depending on the state of charge (SoC), the cell may temporarily be lower after discharge than the applied voltage. After some time, however, it should level off.
During charge, the lead sulfate of the positive plate becomes lead dioxide. As the battery reaches full charge, the positive plate begins generating dioxide causing a sudden rise in voltage due to decreasing internal resistance. A constant voltage charge, therefore, allows detection of this voltage increase and thus control of the current charge amount.

BATTERY CHARGING CHARACTERISTICS​

During constant voltage or taper charging, the battery’s current acceptance decreases as voltage and state of charge increase. The battery is fully charged once the current stabilizes at a low level for a few hours. There are two criteria for determining when a battery is fully charged: (1) the final current level and (2) the peak charging voltage while this current flows.
View attachment 333802
Typical sealed lead acid battery charge characteristics for cycle service where charging is non-continuous and peak voltage can be higher.
View attachment 333803
Typical characteristics for standby service type battery charge. Here, charging is continuous and the peak charge voltage must be lower.

BATTERY CHARGING METHODS​

Selecting the appropriate charging method for your sealed lead acid battery depends on the intended use (cyclic or float service), economic considerations, recharge time, anticipated frequency and depth of discharge (DoD), and expected service life. The goal of any charging method is to control the charge current at the end of the charge.

CONSTANT VOLTAGE CHARGING​

Constant voltage charging is the best method to charge sealed lead acid batteries. Depending on the application, batteries may be charged either on a continuous or non-continuous basis. In applications where standby power is required to operate, for example a security system or uninterruptible power supply (UPS), when the AC power has been interrupted, continuous float charging is recommended. Non-continuous cyclic charging is used primarily with portable equipment where charging on an intermittent basis is appropriate, such as electric wheelchairs and mobile medical carts.
The constant voltage charge method applies a constant voltage to the battery and limits the initial charge current. It is necessary to set the charge voltage according to specified charge and temperature characteristics. Inaccurate voltage settings can cause either over-charge or under-charge. This charging method can be used for both cyclic and standby applications.
View attachment 333800
Constant voltage charging circuit
View attachment 333801
Constant voltage charging characteristics

CONSTANT CURRENT CHARGING​

Constant current charging is suited for applications where discharged ampere-hours of the preceding discharge cycle are known. Charge time and charge quantity can easily be calculated, however an expensive circuit is necessary to obtain a highly accurate constant current. Monitoring of charge voltage or limiting of charge time is necessary to avoid excessive overcharge of the battery.
While this charging method is very effective for recovering the capacity of a SLA battery that has been stored for an extended period of time, or for occasional overcharging to equalize cell capacities, it lacks specific properties required in today’s electronic environment.

TAPER CURRENT CHARGING​

The taper current charging method is not recommended as it is somewhat abusive of sealed lead acid batteries and can shorten service life. However, because of the simplicity of the circuit and low cost, taper current charging is extensively used to charge multiple numbers and/or for cyclic charging.
When using a taper current battery charger the charger time should be limited or a charging cut-off circuit needs to be incorporated to prevent over-charge.
In a taper current charging circuit, the current decreases in proportion to the voltage rise. When designing a taper charger always consider power voltage fluctuations. In this event the internal resistance drop will convert to heat. Heat generated by the circuit should be measured and if required a heat sink should be incorporated in the design.View attachment 333798
Taper current charging circuit
View attachment 333799
Taper current charging characteristics for this type of basically unregulated charger

OVERCHARGING A LEAD ACID BATTERY​

As a result of too high a charge voltage excessive current will flow into the battery, after reaching full charge, causing decomposition of water in the electrolyte and premature aging.
At high rates of overcharge a battery will progressively heat up. As it gets hotter, it will accept more current, heating up even further. This is called thermal runaway and it can destroy a battery in as little as a few hours.

UNDERCHARGING A LEAD ACID BATTERY​

If too low a charge voltage is applied, the current flow will essentially stop before the battery is fully charged. This allows some of the lead sulfate to remain on the electrodes, which will eventually reduce battery capacity.
Batteries which are stored in a discharged state, or left on the shelf for too long, may initially appear to be “open circuited” or will accept far less current than normal. This is caused by a phenomenon called “sulfation”. When this occurs, leave the charger connected to the battery. Usually, the battery will start to accept increasing amounts of current until a normal current level is reached. If there is no response, even to charge voltages above recommended levels, the battery may have been in a discharged state for too long to recover, and in which case a replacement SLA battery will be needed.

LEAD ACID BATTERY CYCLE CHARGING​

Cyclic (or cycling) applications generally require recharging be done in a relatively short time. The initial charge current, however, must not exceed 0.30 x C amps. Just as battery voltage drops during discharge, it slowly rises during charge. Full charge is determined by voltage and inflowing current. When, at a charge voltage of 2.45 ± 0.05 volts/cell, the current accepted by the battery drops to less than 0.01 x C amps (1% of rated capacity), the battery is fully charged and the charger should be disconnected or switched to a float voltage of 2.25 to 2.30 volts/cell. The voltage should not be allowed to rise above 2.45 ± 0.05 volts/cell.

LEAD ACID BATTERY STANDBY CHARGING​

Standby applications generally do not require that the battery be charged as fast or as frequently as in cycle operation. However, the battery must be kept constantly charged to replace the energy that is expended due to internal loss and deterioration of the battery itself. Although these losses are very low in Power Sonic lead acid batteries, they must be replaced at the rate the battery self discharges; at the same time the battery must not be given more than these losses or it will be overcharged. To accomplish this, a constant voltage method of charging called standby or float charging is used.
The recommended constant float voltage is 2.25 – 2.30 volts per cell. Maintaining this float voltage will allow the battery to define its own current level and remain fully charged without having to disconnect the charger from the battery. The trickle current for a fully charged battery floating at the recommended charge voltage will typically hover around the 0.001C rate (7mA for a 7AH battery, for example.)
The float charger is basically a constant voltage power supply. As with cycle chargers, care must be taken not to exceed the initial charge current of 0.30 x C amperes.

TWO STEP CONSTANT VOLTAGE CHARGING​

This method uses two constant voltage devices. In the initial charge phase the high voltage setting is used. When charging is nearly complete and the charge voltage has risen to a specified value (with the charge current decreased), the charger switches the voltage to the lower setting. This method allows rapid charging in cycle or float service without the possibility of overcharging, even after extended charging periods.
View attachment 333804
Dual stage current limited SLA battery charger
View attachment 333805
Two-step constant voltage charging characteristics.

CHARGING 2 OR MORE BATTERIES IN SERIES​

Lead acid batteries are strings of 2 volt cells connected in series, commonly 2, 3, 4 or 6 cells per battery. Strings of lead acid batteries, up to 48 volts and higher, may be charged in series safely and efficiently. However, as the number of batteries in series increases, so does the possibility of slight differences in capacity. These differences can result from age, storage history, temperature variations or abuse.
Fully charged batteries should never be mixed with discharged batteries when charging batteries in series. The discharged batteries should be charged before connection.
When a single constant voltage charger is connected across an entire high voltage string, the same current flows through all cells in the string. Depending on the characteristics of the individual batteries, some may overcharge while others remain in a slightly undercharged condition.
To minimize the effects of individual battery differences, use batteries of the same age, manufacturer, amp hour, and history and, if possible, charge in strings of no greater than 24 or 48 volts.

CHARGING BATTERIES IN PARALLEL​

Lead acid batteries may be used in parallel with one or more batteries of equal voltage. When connecting batteries in parallel, the current from a charger will tend to divide almost equally between the batteries. No special matching of batteries is required. If the batteries of unequal capacity are connected in parallel, the current will tend to divide between the batteries in the ratio of capacities (actually, internal resistances).
When charging batteries in parallel, where different ratios of charge are to be expected, it is best to make provisions to assure that the currents will not vary too much between batteries.

BATTERY TEMPERATURE COMPENSATION​

Power Sonic sealed lead acid batteries perform well both at low and high temperatures. At low temperatures, however, charge efficiency is reduced; at temperatures above 45°C (113°F), charge efficiency increases so rapidly that there is a danger of thermal runaway if temperature compensation is not precise.
The effect of temperature on charge voltage is less critical in float applications than in cyclic use, where relatively high charge currents are applied for the purpose of short recharge times.
Temperature effects should definitely be considered when designing or selecting a charging system. Temperature compensation is desirable in the charging circuit, especially when operating outside the range of 5°C to 35°C
(41°F to 95°F). The temperature coefficient is -2mV/cell/ºC below 20°C (68°F) in float use and -6mV/cell/ ºC below 20°C in cyclic use. For higher temperatures the charge voltage should be correspondingly decreased.
The battery temperature compensation chart below shows the recommended charge voltages for different temperatures based on ambient charge voltage per cell.
TemperatureCyclic Use (V)Float Use (V)
-40°C (-40°F)2.85 – 2.952.38 – 2.43
-20°C (-4°F)2.67 – 2.772.34 – 2.39
-10°C (14°F)2.61 – 2.712.32 – 2.37
0°C (32°F)2.55 – 2.652.30 – 2.35
10°C (50°F)2.49 – 2.592.28 – 2.33
20°C (68°F)2.43 – 2.532.26 – 2.31
25°C (77°F)2.40 – 2.502.25 – 2.30
30°C (86°F)2.37 – 2.472.24 – 2.29
40°C (104°F)2.31 – 2.412.22 – 2.27
50°C (122°F)2.25 – 2.352.20 – 2.25

TOP UP CHARGING SLA BATTERIES​

All batteries lose capacity through self-discharge, it is recommended that a “top up charge” be applied to any battery that has been stored for a long period of time, prior to putting the battery into service.
To successfully top up charge a battery stored for more than 12 months, the open circuit voltage must be higher than 2.0 volts per cell, in this case, always confirm open circuit voltage prior to attempting top up charging.

BATTERY CHARGING EFFICIENCY​

The charging efficiency (η) of a battery is expressed by the following formula:View attachment 333806
The charging efficiency varies depending upon the state of charge of the battery, temperatures, and charging rates. The below graph illustrates the concept of the state of charge and charging efficiency.
The below graph shows Power Sonic sealed lead acid batteries exhibit very high charging efficiency, even when charged at low charging rates.
View attachment 333807
It is always important to match your charger to deliver the correct current and voltage for the battery you are charging. For example, you wouldn’t use a 24V charger to charge a 12V battery.


amberwolf, thanks for your reply with the information for charging lead acid battery.

I understand that AGM battery is a kind of lead acid battery. But there are chargers/charger settings which are specially for AGM batteries. Are there any other information/precautions that I should note when charging AGM battery with my current equipment?
 
I have an odyssey 3 year old 16ah agm and also a 11 year old fullriver full throttle 27ah agm. I just charge them as a regular lead acid battery constant voltage/constant current at 3 amps. The only thing you need to pay attention too is the recommended bulk voltage. Some high performance agm's need 14.7 volts instead of the normal 14.4 volts when bulk charging.
I used to have a 100ah kinitek agm battery as a house battery. I was charging with solar and due to voltage drop it never charged above 14 volts (solar controller read 14.4 volts) . The chronic undercharging eventually destroy the battery. Once the battery got below 11 volts 1 or 2 times it usually loses capacity. It will charge up quickly to 14.4 volts but once you put a load on it, it doesnt last long.

If your power supply is cc/cv it should work in charging the battery, I would set the max voltage to 14.4 volts, and just watch the amps, when it reaches 14.4 volts and the amps drop to 100ma or less its usually fully charge. 4 amps is a good charge rate since the condition of the battery is unknowned. You just need to charge it more than 6 hours, 4 amps x 6 hours = 24 ah, since the starting voltage was 11.17 volts (12.1 volts is 50 percent) that means the battery is nearly empty (below 10 percent) , you need to put at least 90 ah back into the battery to get it up to 14.4 volts. The 6 hours of charging only got it up to 11.97, it needs more charging. Once you disconnect the charger, the battery voltage drops to the true battery voltage. A good battery fully charged to 14.4 volts will drop to about 12.7 volts when disconnected from the charger.

a 12 volt batt  soc.jpg
 
I have an odyssey 3 year old 16ah agm and also a 11 year old fullriver full throttle 27ah agm. I just charge them as a regular lead acid battery constant voltage/constant current at 3 amps. The only thing you need to pay attention too is the recommended bulk voltage. Some high performance agm's need 14.7 volts instead of the normal 14.4 volts when bulk charging.
I used to have a 100ah kinitek agm battery as a house battery. I was charging with solar and due to voltage drop it never charged above 14 volts (solar controller read 14.4 volts) . The chronic undercharging eventually destroy the battery. Once the battery got below 11 volts 1 or 2 times it usually loses capacity. It will charge up quickly to 14.4 volts but once you put a load on it, it doesnt last long.

If your power supply is cc/cv it should work in charging the battery, I would set the max voltage to 14.4 volts, and just watch the amps, when it reaches 14.4 volts and the amps drop to 100ma or less its usually fully charge. 4 amps is a good charge rate since the condition of the battery is unknowned. You just need to charge it more than 6 hours, 4 amps x 6 hours = 24 ah, since the starting voltage was 11.17 volts (12.1 volts is 50 percent) that means the battery is nearly empty (below 10 percent) , you need to put at least 90 ah back into the battery to get it up to 14.4 volts. The 6 hours of charging only got it up to 11.97, it needs more charging. Once you disconnect the charger, the battery voltage drops to the true battery voltage. A good battery fully charged to 14.4 volts will drop to about 12.7 volts when disconnected from the charger.

View attachment 333835
jonyjoe303, thanks for your reply and suggestions.
For the bubbling of just one cells, when I used the trickle charger to charge the battery, there is no bubbling in all cells. Do you suggest to lower the charging current (below 4A) to avoid further damage to that cell? According to amberwolf, bubbling is not normal. But, I remember I used to add water to my car battery (not this AGM battery) and charged it with my trickle charger occasionally, and all cells would bubble. That car and battery was 13 years old and still function good when I traded it in. Do you think we should try to avoid bubbling when charging?
 
The VR means valve regulated, and AGM is absorbed glass mat.
I doubt it's a charging problem. It sounds like a putting water in a dried out gel battery that probably has popped overpressure vents problem.
What makes an AGM charger different is it doesn't go to as high a voltage as regular lead acid, which needs the volts to drive the charge deep into the lead plates.
But on AGM the high volts dries out the mats and pops the vents, esp if someone tried an equalizing setting on it like a regular lead acid can handle, but AGM can't.
 
Last edited:
If only one cell is bubbling, it likely indicates one or more of the other cells is partially shorted. This can happen when the battery is overdischarged and left sitting for a long time. Sulfate can build up enough to squeeze the plate separators to the point they puncture or there is a conductive bridge formed around the edges of the separators. I have not had much luck recovering batteries in this condition. A pulse charger left running long enough may break down the sulfate somewhat but if there is a short or partial short, it is pretty hopeless.
 