Cycle life tests of High Energy density cylindrical cells

Small update

Update:
- added more cycles at 90% and 100%.
- Samsung "58E" begins to die after 600 cycles at 100% DoD :( a similar fate is waiting for the Samsung 53G1. I would recommend to wait for the "2" generation, which is common rule in Samsung production line.

More to come:
Vapcell F63, N41 and finally LG M52VT are on the way to me.
 
Greetings! I previously wrote a review on the elements of FEB 6000mah (vapcell f60). I built a 16s14p battery. At a constant load of 60 amps, the battery overheated. In the end, I still put the battery on my electric bike. I'm taking 80 amps off it at its peak and there wasn't any overheating, not even close) I have gear motor wheels in all-wheel drive and it is problematic to keep almost 5 kW of power on them at all times ..) Although I drive extremely aggressively. Initially, the battery is assembled on FEB 6000 mAh cells. I'm currently building the same one on a Vapcell f60. When analyzing FEB and Vapcell, I saw the difference. Apparently, they produce batches for Vapcell separately on FEB, because Vapcell has clearly better characteristics and they do not heat up so much
 
Greetings! I previously wrote a review on the elements of FEB 6000mah (vapcell f60). I built a 16s14p battery. At a constant load of 60 amps, the battery overheated. In the end, I still put the battery on my electric bike. I'm taking 80 amps off it at its peak and there wasn't any overheating, not even close) I have gear motor wheels in all-wheel drive and it is problematic to keep almost 5 kW of power on them at all times ..) Although I drive extremely aggressively. Initially, the battery is assembled on FEB 6000 mAh cells. I'm currently building the same one on a Vapcell f60. When analyzing FEB and Vapcell, I saw the difference. Apparently, they produce batches for Vapcell separately on FEB, because Vapcell has clearly better characteristics and they do not heat up so much
Thank you for posting your experiences with these cells!

It’s rare to have the same cell, even of different grades, perform so differently like that. And FEB would never sell “better” cells to a company as small as Vapcell instead of to their huge commercial customers (buying millions of cells a year). If anything, Vapcell would get the same cells or even a lower grade since they wouldn’t be a prime customer for the top grade cells.

I know it was the rumor that was going around but has it actually been confirmed that the F60 uses the FEB 6Ah cell? Have you compared the cells (with wraps off) and they are identical in appearance, even when using a magnifier?
 
This is a good question. I still have no confirmation who is the manufacturer of the F60 series from Vapcell. It was my speculation that FEB might be the manufacturer, because at that time I had no information about any other manufacturer that had 6000 mAh cells in their lineup.
Also, to this day I have not been able to obtain samples of the original FEB cells for comparison. One of the distributors just told me that they have already removed FEB cells from their stock because customers complained about their quality. Since Vapcell now has F63 and FEB doesn't have anything like that on the site, I would be more inclined to think that Vapcell is getting cells from another manufacturer.
 
This is a good question. I still have no confirmation who is the manufacturer of the F60 series from Vapcell. It was my speculation that FEB might be the manufacturer, because at that time I had no information about any other manufacturer that had 6000 mAh cells in their lineup.
Also, to this day I have not been able to obtain samples of the original FEB cells for comparison. One of the distributors just told me that they have already removed FEB cells from their stock because customers complained about their quality. Since Vapcell now has F63 and FEB doesn't have anything like that on the site, I would be more inclined to think that Vapcell is getting cells from another manufacturer.
Another supplier of the FEB 6000mAh cell did tell me that FEB might have done some naughty things around the cell's release regarding battery grades.

Apparently, most of those cells on the market are actually B-grade currently, and only recently have true A-grade cells been a thing; FEB/FST's definition of A-grade for this cell might have changed with time to increase valuable yields.
 
Another supplier of the FEB 6000mAh cell did tell me that FEB might have done some naughty things around the cell's release regarding battery grades.
I’d be stunned if that was true as it would be ”corporate suicide”. Their large customers would drop them quickly and buy from another manufacturer rather than deal with the nightmare of changing cell performance…IMHO.

But in the cutthroat world that is cell manufacturing, especially when China gets involved, I guess we can never say never.

Apparently, most of those cells on the market are actually B-grade currently, and only recently have true A-grade cells been a thing; FEB/FST's definition of A-grade for this cell might have changed with time to increase valuable yields.
I completely agree that many, even most, of the cells we buy are likely not top grade. At least until demand drops for the top grade cells or the big customers start selling off excess top grade inventory.

We are in the terrible situation of only being able to get info via rumors and (almost) never having access to known top grade cells to use as a performance reference when testing. Incredibly frustrating!
 
I’d be stunned if that was true as it would be ”corporate suicide”. Their large customers would drop them quickly and buy from another manufacturer rather than deal with the nightmare of changing cell performance…IMHO.

But in the cutthroat world that is cell manufacturing, especially when China gets involved, I guess we can never say never.


I completely agree that many, even most, of the cells we buy are likely not top grade. At least until demand drops for the top grade cells or the big customers start selling off excess top grade inventory.

We are in the terrible situation of only being able to get info via rumors and (almost) never having access to known top grade cells to use as a performance reference when testing. Incredibly frustrating!
Of course, but there's the corporations' market, and then there's the small business market.

I wouldn't be surprised "smaller" companies like FEB prioritize the highest grade cells for those who order 500k+ cells to millions of cells every year, and then we got the "scraps" for a while.

But yeah, this kind of informed speculation is killing.

If I was rich, I'd just pose as a large customer and try to extract blood from the stones, but even then, I doubt I'd get the answers we want.

In the meantime, I can now order EVE 50PLs :D
Perfect cold weather cells, although they're 2x more expensive than 50Es.
 
Of course, but there's the corporations' market, and then there's the small business market.

I wouldn't be surprised "smaller" companies like FEB prioritize the highest grade cells for those who order 500k+ cells to millions of cells every year, and then we got the "scraps" for a while.

But yeah, this kind of informed speculation is killing.

If I was rich, I'd just pose as a large customer and try to extract blood from the stones, but even then, I doubt I'd get the answers we want.

In the meantime, I can now order EVE 50PLs :D
Perfect cold weather cells, although they're 2x more expensive than 50Es.
50PL where, I need to know :)
 
Something something Alibaba supplier send me a message that they're now available if I'm willing to pay 15-20% extra than the BAK 45Ds I've been eyeing.

Awesome, I hope they pop up on nkon soon. I need 40 pcs for some battery packs. Shipping from China would probably make them too expensive.
 
The person who cooked the battery cut both elements. The element from Vapcell is different from FEB. Despite the fact that I contacted Vapcell directly and asked them about the manufacturer of the elements. They said about FEB. And about the fact that the grade was B... I highly doubt it. I agree that the company would have buried its reputation, because there is high competition in the market and such stupid steps would have hurt the company.
 
I would be very interested to see also some older cells, which you tested, I guess, LG MJ 18650 or Sanyo NCR 18650GA. But only if you have already the results.

In one of the threads you @Pajda wrote, that you want to make a new thread for the best price/value cells. I think that would be very useful.
 
In one of the threads you @Pajda wrote, that you want to make a new thread for the best price/value cells. I think that would be very useful.

Yes, this idea came up some time ago when I publicly complained that there are almost no new products on the market to test. Well, since this forum is followed daily by all the big cell manufacturers :) , they couldn't let it go and a shitstorm of announced news appeared. Which brought me back to my original motivation of testing the best current technologies regardless of price.
 
I found an interesting post on linkedin, I'm a bit late to the party with the post being over a month old but this was the first time I've heard of this cell so I thought I would share. Molicel M64A. 6.4ah and a claimed 25A max discharge, personally I'm glad to see the super high energy cells haven't been left in the dust with these new high power cells coming out. On the post it's stated to enter mass production in Q3 25', and the poster can help book samples (to me it wasn't clear if they were available now).
 

Attachments

  • 1747178246172.png
    1747178246172.png
    267.6 KB · Views: 21
I found an interesting post on linkedin, I'm a bit late to the party with the post being over a month old but this was the first time I've heard of this cell so I thought I would share. Molicel M64A. 6.4ah and a claimed 25A max discharge, personally I'm glad to see the super high energy cells haven't been left in the dust with these new high power cells coming out. On the post it's stated to enter mass production in Q3 25', and the poster can help book samples (to me it wasn't clear if they were available now).
Interesting!
i haven’t heard about it and it’s not mentioned in their 2024 annual report (recent cell developments).
 
Interesting!
i haven’t heard about it and it’s not mentioned in their 2024 annual report (recent cell developments).
Interesting, I figured you already had but couldn't share it with us (like a possible nda situation), only reason I didn't put it in the patreon. I guess add it to the list of cells to try to get samples of and test! :LOL:
 
Two cells were added to BAK's website then removed (?):

N21700CX-65E
N21700CX-71E

1. N21700CX-65E
  • Electrical Specifications:
    • Typical Capacity: 6.5 Ah (0.2C)
    • Nominal Voltage: 3.5 V
    • Internal Resistance: ≤10 mΩ
    • Max Discharge Rate: 2C
    • Max Charge Rate: 1C
    • Cycle Life & Operating Conditions:
    • Cycle Life: 500 cycles > 80% (100% DOD, 25°C, RT0.5C/1C)
    • Operating Temperature Range (Cell Surface):
      • Charge: -20 to 70°C
2. N21700CX-71E
  • Electrical Specifications:
    • Typical Capacity: 7.1 Ah (0.2C)
    • Nominal Voltage: 3.5 V
    • Internal Resistance: ≤10 mΩ
    • Max Discharge Rate: 2C
    • Max Charge Rate: 1C
  • Cycle Life & Operating Conditions:
    • Cycle Life: 500 cycles > 80% (100% DOD, 25°C, 0.5C/1C)
    • Operating Temperature Range (Cell Surface):
      • Charge: -20 to 70°C
 
Two cells were added to BAK's website then removed (?):

N21700CX-65E
N21700CX-71E

And here we go again. You are excited that the market situation has calmed down for a while and you are slowly catching up with the testing of 5800mAh+ cells and then @Souvlucky will be back :cool: , right away with a 7.1Ah cell? 1025 Wh/l like seriously?
 
Interesting, along with 3.5V nominal voltage, something a bit different :)
High silicon anode rearing its head once again.

I don't think my heart can take the possibility of getting anywhere near close to the theoretical energy density limit (around 3.3kWh/kg for a full cell).

At this point, I'm expecting 700Wh/kg cells to appear next year, 800Wh/kg in 2027, 1000Wh/kg in 2030 and 2000Wh/kg in 2040.
 