Pajda
10 kW
"Standard Power Rate" test (1C continuous discharge)
note: the 1C discharge test is performed at ca 90% DoD (4.15V-3.00V)
Test eqiupment:
- 2pcs ZKETECH EBC-X0510
- BF-2A four-wire cell fixture (10A version with Nickel plated contacts)
- tested in room with relatively stable temperature 23 ±2 °C
Remarks and comments:
- someone considers these testers a child's toy
- the most problematic is tester accuracy. It is 0.2 % ±0.01 A. The stability is relatively good.
- do not much look at the absolute values, particularly at low currents in nominal capacity tests, trends are here important results.
- will try to add more data as it will come
- each 50th cycle is inserted datasheet nominal capacity test with 10s DCIR test (see dots in figure)
- minimal charging CV phase cut-off current is set to 100 mA due to the ZKETECH testers limitation
____
"Table" with values measured on precision battery tester (not ZKETECH). Those test were performed in temperature chamber under 25°C, TC is using forced air flow to maintan consistent temp. This 25°C air flow acts as cooling force on the cell surface, so the measured temperatures under high load will be affected by this.
added Samsung 30Q6 to the chart (X0510 tester), sample source: ---
added Sony 18650VTC6 to the chart (X0510 tester), sample source: NKON
added Samsung INR21700-40T3 to the chart (A20 tester), , sample source: NKON
added Samsung INR21700-50S(1) to the chart (A20 tester), sample source: NKON
added Molicel INR21700-P42A to the chart (X0510 tester), sample source: NKON
added Molicel INR21700-P45B to the chart (X0510 tester), sample source: NKON
added Molicel INR18650-HJ2 to the chart (X0510 tester), sample source: Vapcell
added Tenpower INR21700-40TG to the chart (X0510 tester), sample source: NKON
added Samsung INR21700-40T4 to the chart (A20 tester), , sample source: Vapcell
note: the 1C discharge test is performed at ca 90% DoD (4.15V-3.00V)
Test eqiupment:
- 2pcs ZKETECH EBC-X0510
- BF-2A four-wire cell fixture (10A version with Nickel plated contacts)
- tested in room with relatively stable temperature 23 ±2 °C
Remarks and comments:
- someone considers these testers a child's toy
- the most problematic is tester accuracy. It is 0.2 % ±0.01 A. The stability is relatively good.
- do not much look at the absolute values, particularly at low currents in nominal capacity tests, trends are here important results.
- will try to add more data as it will come
- each 50th cycle is inserted datasheet nominal capacity test with 10s DCIR test (see dots in figure)
- minimal charging CV phase cut-off current is set to 100 mA due to the ZKETECH testers limitation
____
"Table" with values measured on precision battery tester (not ZKETECH). Those test were performed in temperature chamber under 25°C, TC is using forced air flow to maintan consistent temp. This 25°C air flow acts as cooling force on the cell surface, so the measured temperatures under high load will be affected by this.
added Samsung 30Q6 to the chart (X0510 tester), sample source: ---
added Sony 18650VTC6 to the chart (X0510 tester), sample source: NKON
added Samsung INR21700-40T3 to the chart (A20 tester), , sample source: NKON
added Samsung INR21700-50S(1) to the chart (A20 tester), sample source: NKON
added Molicel INR21700-P42A to the chart (X0510 tester), sample source: NKON
added Molicel INR21700-P45B to the chart (X0510 tester), sample source: NKON
added Molicel INR18650-HJ2 to the chart (X0510 tester), sample source: Vapcell
added Tenpower INR21700-40TG to the chart (X0510 tester), sample source: NKON
added Samsung INR21700-40T4 to the chart (A20 tester), , sample source: Vapcell
Attachments
-
HP_1C_cycle_life_test@voltage_drop_new.png231.7 KB · Views: 2,203
-
HP_1C_cycle_life_test@voltage_drop_1000cycle.png165.1 KB · Views: 2,040
-
HP_1C_cycle_life_test@temperature_new.png156 KB · Views: 1,964
-
HP_1C_cycle_life_test@temperature_1000cycle.png145.3 KB · Views: 1,964
-
HP_3C_cycle_life_test@voltage_drop_new.png184.8 KB · Views: 1,991
-
HP_3C_cycle_life_test@voltage_drop_1000cycle.png153.7 KB · Views: 1,969
-
HP_3C_cycle_life_test@temperature_new.png193.6 KB · Views: 1,957
-
HP_3C_cycle_life_test@temperature_1000cycle.png159.9 KB · Views: 1,991
-
HP_1C_cycle_life_test@DCIR10s rise.png217.4 KB · Views: 655
-
HP_1C_cycle_life_test@capacity_drop.png263.1 KB · Views: 683
Last edited: