JP spot-welder, FET-switched, timed adj. pulse

any idea?.
both red and green LED work as they should.

Mosfet test infinite in one direction and about 6Mohms on the other... i get 0.442V in diode test mode and infinite with the other polarity..

but i get 12V continuous at the probe leg ( they conduct all the time!)

Does the mosfet driver could make mosfet to conduct when there is a little current between drain and source?

Doc
 
Doctorbass said:
any idea?.
both red and green LED work as they should.

Mosfet test infinite in one direction and about 6Mohms on the other... i get 0.442V in diode test mode and infinite with the other polarity..

but i get 12V continuous at the probe leg ( they conduct all the time!)

Does the mosfet driver could make mosfet to conduct when there is a little current between drain and source?

Doc

Make sure the JP Welder side is connected to negative pole of battery. If they're reversed, you'll have this exact condition.
 
that1guy said:
Decided to jump in the tab welder game.

Specs:
8x 0.11F (rated), 0.15F (measured), 15V ALEL caps => 120J
6x IRFP4004 MOSFETS, 40V, 1.35mΩ
6.35mm thick Al busbars


Any more pictures, this looks rad.

Did you mill the traces or use a photoresist? Any plans to sell kits/opensource? Voltage or discharge time adjustments?
 
VirgilBudBrigman said:
Doctorbass said:
any idea?.
both red and green LED work as they should.

Mosfet test infinite in one direction and about 6Mohms on the other... i get 0.442V in diode test mode and infinite with the other polarity..

but i get 12V continuous at the probe leg ( they conduct all the time!)

Does the mosfet driver could make mosfet to conduct when there is a little current between drain and source?

Doc

Make sure the JP Welder side is connected to negative pole of battery. If they're reversed, you'll have this exact condition.


lol.. no they are in the right polarity...

problem seem deeper than that...

but i have found.. when the PIC blew, all mosfet switched ON continuously and melted the 10gauge wire that i had shorted to the probes... now when i apply 12V all mosfet are " ON" and have about 4 volt between drain and source... i'll replace them all

Doc
 
adriftatsea said:
that1guy said:
Decided to jump in the tab welder game.

Specs:
8x 0.11F (rated), 0.15F (measured), 15V ALEL caps => 120J
6x IRFP4004 MOSFETS, 40V, 1.35mΩ
6.35mm thick Al busbars


Any more pictures, this looks rad.

Did you mill the traces or use a photoresist? Any plans to sell kits/opensource? Voltage or discharge time adjustments?

Traces were milled with cnc machine.

Not pictured is a Teensy board that controls the show. I send it a request for via serial port for X energy on the caps. The Teensy charges or discharges caps to a voltage corresponding to E=1/2 * C * V^2. Pulse timing is also set via serial port. There's a weld pedal input pin, but that's also controllable via serial port.

I wouldn't mind open sourcing it once it's a bit more polished. I wonder how many people actually want to build a welder themselves with caps that have this same terminal spacing and threads.

I also made a spring loaded weld head. This part might be of more interest to the community.
e2TCHiE.png
 
I LOVE COPPER ! 8)

Here is the update on my build: (as well you will notice that the JP spotwelder is not there yet.. i need to replace all fets! :lol: i blown their gate when shorted them to too much copper :lol: it will be installed on the left of teh first picture you see on the top NEG bus bar from the caps.

The big copper bar you see is one of the two output lead of the system. These will be MASSIVE for maximum current!

-1.25" x 0.25" thick pure copper bus rail for high current connections from teh caps modules to the output tabs of the welder
-high quality industrial ultraflexible TRUE pure copper 4 gauge cable
-3/8" dia pure copper tip holder with fixing dual 8-32 set screw
-1/8" dia x 1" tungsten tip for copper spotweldfing

The measured total resistance of the system including the contact resistance on a 6 mil x 10mm wide copper sheet at distance of 5mm and capacitor ESR is only 2.0 miliohms.

And!...Total measured caps ESR is 0.12 miliohms. Enough for a 100 000Amps short at 12v :twisted: but that copper would vaposize in fract of a second before reaching that as well!

Total energy stored is 0.5Wh at max 35V ( close to 2kJ)

The highest resistance of the system will be between the two tips! :wink:

Doc
 

Attachments

  • 20160517_000228 (Personnalisé)1.jpg
    20160517_000228 (Personnalisé)1.jpg
    76.3 KB · Views: 5,764
  • 20160517_000212 (Personnalisé)1.jpg
    20160517_000212 (Personnalisé)1.jpg
    85.8 KB · Views: 5,764
  • 20160517_000101 (Personnalisé)1.jpg
    20160517_000101 (Personnalisé)1.jpg
    76.8 KB · Views: 5,764
  • 20160516_235736_Richtone(HDR) (Personnalisé)1.jpg
    20160516_235736_Richtone(HDR) (Personnalisé)1.jpg
    42.3 KB · Views: 5,764
  • 20160515_144429 (Personnalisé)1.jpg
    20160515_144429 (Personnalisé)1.jpg
    60.6 KB · Views: 5,764
  • 20160515_145045 (Personnalisé)1.jpg
    20160515_145045 (Personnalisé)1.jpg
    75 KB · Views: 5,764
  • 20160516_235636_Richtone(HDR) (Personnalisé)1.jpg
    20160516_235636_Richtone(HDR) (Personnalisé)1.jpg
    54.6 KB · Views: 5,764
okashira said:
Finally. Did a before and after fully quantifying the effect of the flyback diode. Further, Added a TVS diode and I was able to completely prevent avalanche!


SOURCE-DRAIN VOLTAGE @ MOSFET TURN OFF
All are done at welding current of about 2,500 amps.
1.) WHITE - no diode - 110 microseconds of avalanche, peak voltage of 30.5V across FET's
2.) ORANGE - flyback diode added - 20 microseconds of avalanche, peak voltage of 29V across FET's
3.) YELLOW - TVS diode added - zero avalanche - peak voltage of ~21V
tEDxoJE.jpg


One way I really found out that the flyback is doing most of the work. I tried the TVS diode alone, and it immediatly blew the leg of the TVS diode on the first pulse. It's fine with the flyback there.
s20i9WK.jpg





TEST SETUP
cfaUH4t.jpg

I'm confused here, is there currently something better than using that huge schottky diode that you were using originally? That is what I'm using right now.
 
Finished spot-welding 240 cells (20S12P from 5 separate 4S12P packs, LG HG2 cells, 3000mAh/ea, 20A continuous each, total of 2.6kwh). Used 0.2mm x 8mm pure nickel, carefully laid out to achieve approximately 160-170A ampacity.

JP Welder has not been perfect, but I got through it! I blew a trace and a mosfet, but I put that down to the several feet of 1GA welding wire I originally used to extend from the car to the table. Later replaced all the MOSFETS with same type but automotive grade (like another $1-2 total, why not!?). Also implemented the diode mod (VS­100BGQ045) that Okashira recommended. Of course, I also stopped using the long wires (less resistance) and implemented other mods, like the cooling fan and 12GA romex wire from the bus-bar to the MOSFETS. The whole thing runs VERY cool now, used to get almost burning hot! (Only the tips of the electrodes get warm when doing rapid fire welds)

The biggest issue I had (and a scary one) was several dozen times I had blowouts (craters), which are quite scary! My material is pure nickel and I experimented with differing pressure, timings, angle, cleaning the electrodes constantly, etc. I'm thinking the copper electrode material of these is not ideal...there must be something better! Furthermore, the wires themselves are not flexible at all...so I'm glad to see others looking to rectify these issues.

Another issue was sticking, and some of the copper getting left in the weld. This happened for up to half of all the welds. I tried the press and rotate technique others spoke of...which helps some. The sticking seems to contribute to the breakdown of the electrode, and needing to un-screw, put in the drill and spin it smooth and round/pointy again. I also lowered the settings down until pulling hard would "just" not break free of the cell.

I used a single brand-new Rural King battery (same as Exide Edge for a little more than 1/2 the cost, my wife's car battery had just died so the timing was perfect! http://www.ruralking.com/battery-auto-agm-rk-agm24f.html) and it worked VERY well. Before the mods I was up to 2/3 or so on the dial. After the mods, I was down to under 1/3 on the dial. Don't assume that you will need two batteries, for a good battery and 0.2mm nickel, you probably need only one!

SUMMARY: This spot-welding business is not for the faint of heart. Ironically, it's also not for the careless! Biggest improvements (post-mods) would be better electrode material and more flexible welding cables. (Or go with Headways if they dramatically improve the chemistry and you can fit them! :p )
 

Attachments

  • IMG_20160515_150506.jpg
    IMG_20160515_150506.jpg
    263.7 KB · Views: 5,741
  • IMG_20160515_010203.jpg
    IMG_20160515_010203.jpg
    141.3 KB · Views: 3,151
  • IMG_20160510_204106.jpg
    IMG_20160510_204106.jpg
    144.1 KB · Views: 3,149
  • IMG_20160507_135423.jpg
    IMG_20160507_135423.jpg
    234.7 KB · Views: 5,742
  • IMG_20160507_135415.jpg
    IMG_20160507_135415.jpg
    266.4 KB · Views: 5,743
  • IMG_20160507_134642.jpg
    IMG_20160507_134642.jpg
    175.3 KB · Views: 5,743
Really cool and impressive builds posted recently!

My findings on electrodes sticking may not apply to too many configurations out there but I thought I post them just in case it helps someone out of new things to try to resolve it.
I did not have much sticking problem with 0.15 mm pure nickel but when I went to 0.20 (also pure nickel) all hell broke loose; it was sticking so bad it looked like it was designed to do so.
Someone on the board mentioned cutting a slit on the nickel and I tried that. It really worked in my case and I am finishing a jig with an abrasive cutting wheel from Dremel, 0.025 inch thick, that will allow me to quickly cut just the perfect size slit on the nickel strip wherever I need it.
I will post some pictures in a day or two.
 
Doctorbass said:
I LOVE COPPER ! 8)

Here is the update on my build: (as well you will notice that the JP spotwelder is not there yet.. i need to replace all fets! :lol: i blown their gate when shorted them to too much copper :lol: it will be installed on the left of teh first picture you see on the top NEG bus bar from the caps.

The big copper bar you see is one of the two output lead of the system. These will be MASSIVE for maximum current!

-1.25" x 0.25" thick pure copper bus rail for high current connections from teh caps modules to the output tabs of the welder
-high quality industrial ultraflexible TRUE pure copper 4 gauge cable
-3/8" dia pure copper tip holder with fixing dual 8-32 set screw
-1/8" dia x 1" tungsten tip for copper spotweldfing

The measured total resistance of the system including the contact resistance on a 6 mil x 10mm wide copper sheet at distance of 5mm and capacitor ESR is only 2.0 miliohms.

And!...Total measured caps ESR is 0.12 miliohms. Enough for a 100 000Amps short at 12v :twisted: but that copper would vaposize in fract of a second before reaching that as well!

Total energy stored is 0.5Wh at max 35V ( close to 2kJ)

The highest resistance of the system will be between the two tips! :wink:

Doc
keen to see the results Doc, those tungsten tips are a work of art!
 
VirgilBudBrigman said:
Finished spot-welding 240 cells (20S12P from 5 separate 4S12P packs, LG HG2 cells, 3000mAh/ea, 20A continuous each, total of 2.6kwh). Used 0.2mm x 8mm pure nickel, carefully laid out to achieve approximately 160-170A ampacity.

JP Welder has not been perfect, but I got through it! I blew a trace and a mosfet, but I put that down to the several feet of 1GA welding wire I originally used to extend from the car to the table. Later replaced all the MOSFETS with same type but automotive grade (like another $1-2 total, why not!?). Also implemented the diode mod (VS­100BGQ045) that Okashira recommended. Of course, I also stopped using the long wires (less resistance) and implemented other mods, like the cooling fan and 12GA romex wire from the bus-bar to the MOSFETS. The whole thing runs VERY cool now, used to get almost burning hot! (Only the tips of the electrodes get warm when doing rapid fire welds)

The biggest issue I had (and a scary one) was several dozen times I had blowouts (craters), which are quite scary! My material is pure nickel and I experimented with differing pressure, timings, angle, cleaning the electrodes constantly, etc. I'm thinking the copper electrode material of these is not ideal...there must be something better! Furthermore, the wires themselves are not flexible at all...so I'm glad to see others looking to rectify these issues.

Another issue was sticking, and some of the copper getting left in the weld. This happened for up to half of all the welds. I tried the press and rotate technique others spoke of...which helps some. The sticking seems to contribute to the breakdown of the electrode, and needing to un-screw, put in the drill and spin it smooth and round/pointy again. I also lowered the settings down until pulling hard would "just" not break free of the cell.

I used a single brand-new Rural King battery (same as Exide Edge for a little more than 1/2 the cost, my wife's car battery had just died so the timing was perfect! http://www.ruralking.com/battery-auto-agm-rk-agm24f.html) and it worked VERY well. Before the mods I was up to 2/3 or so on the dial. After the mods, I was down to under 1/3 on the dial. Don't assume that you will need two batteries, for a good battery and 0.2mm nickel, you probably need only one!

SUMMARY: This spot-welding business is not for the faint of heart. Ironically, it's also not for the careless! Biggest improvements (post-mods) would be better electrode material and more flexible welding cables. (Or go with Headways if they dramatically improve the chemistry and you can fit them! :p )

I think the craters you are talking about is when you dont have a solid connection under the nickeltab. Like when you are slightly beside the positive terminal of the cell. I had the same craters, but didnt really weld after that occation, to see if I actually was "missing" the positive terminal. Someone in this thread had this idea.
 
Here are the pics of the jig I made to allow me to quickly (literately, about 2 seconds) and consistently cut a slit on the nickel strip.
I know it looks over the top but I had this wonderful phenolic material and a Weecher rotary tool with a straight wand that is great for holding it in a similar fashion as a chop saw.

I know they sell some nickel already slitted but I don't like its width and thickness and at least the one I bought is not pure nickel.

The mandrel is mounted in a swinging support with two springs to push it up and allow the positioning of the strip in the slot that is exactly the width of the nickel. Then a quick push down and a slit is form, allowing for a weld with less sticking electrodes.
 

Attachments

  • IMG_2473.JPG
    IMG_2473.JPG
    90.2 KB · Views: 5,627
  • IMG_2479.JPG
    IMG_2479.JPG
    94.2 KB · Views: 5,627
  • IMG_2483.JPG
    IMG_2483.JPG
    55.3 KB · Views: 5,625
  • IMG_2488.JPG
    IMG_2488.JPG
    75.5 KB · Views: 5,625
Heres a question for the engineers in the group. How can I determine the root cause of my FET failures.

FETs blow either because of too much forward current during the weld time, or two much reverse current (avalanche) at pulse turn off. So from what I've read here you can:
Lower the forward current/shorten the weld time (lower FET heating) with 1. lower Rds on FETs, 2. lower voltage battery supply, 3. higher resistance (longer or smaller gauge power leads.)
Lower the avalanche current that the FETs see with 4. shorter non coiled weld leads (less inductance), 5. add a snubber diode. 6. add and RC snubber that lowers peak avalanche current but maybe not much lower energy.

Now then - how can I tell which of the above to do first when I want to keep my FETs from smoking. How can I tell if it was a forward or avalanche current failure .
Thanks for all feedback.
 
Geekineer said:
Heres a question for the engineers in the group. How can I determine the root cause of my FET failures.

FETs blow either because of too much forward current during the weld time, or two much reverse current (avalanche) at pulse turn off. So from what I've read here you can:
Lower the forward current/shorten the weld time (lower FET heating) with 1. lower Rds on FETs, 2. lower voltage battery supply, 3. higher resistance (longer or smaller gauge power leads.)
Lower the avalanche current that the FETs see with 4. shorter non coiled weld leads (less inductance), 5. add a snubber diode. 6. add and RC snubber that lowers peak avalanche current but maybe not much lower energy.

Now then - how can I tell which of the above to do first when I want to keep my FETs from smoking. How can I tell if it was a forward or avalanche current failure .
Thanks for all feedback.


You are probably using too powerful battery. You should use diode or smaller battery :)
 
Geekineer said:
Heres a question for the engineers in the group. How can I determine the root cause of my FET failures.

FETs blow either because of too much forward current during the weld time, or two much reverse current (avalanche) at pulse turn off. So from what I've read here you can:
Lower the forward current/shorten the weld time (lower FET heating) with 1. lower Rds on FETs, 2. lower voltage battery supply, 3. higher resistance (longer or smaller gauge power leads.)
Lower the avalanche current that the FETs see with 4. shorter non coiled weld leads (less inductance), 5. add a snubber diode. 6. add and RC snubber that lowers peak avalanche current but maybe not much lower energy.

Now then - how can I tell which of the above to do first when I want to keep my FETs from smoking. How can I tell if it was a forward or avalanche current failure .
Thanks for all feedback.

What welder are you using?
 
Hi....its a home brew but very similar to J P with 1407 driver chip and 6 parallel 1324 fets. Twice blew F E T closest to driver. All pins shorted and drain lead fused. Need to replace all six I guess and add external avalanche diode. Trying to understand root cause of failure...avalanche or over limit forward current/time.
 
that1guy said:
adriftatsea said:
that1guy said:
Decided to jump in the tab welder game.

Specs:
8x 0.11F (rated), 0.15F (measured), 15V ALEL caps => 120J
6x IRFP4004 MOSFETS, 40V, 1.35mΩ
6.35mm thick Al busbars


Any more pictures, this looks rad.

Did you mill the traces or use a photoresist? Any plans to sell kits/opensource? Voltage or discharge time adjustments?

Traces were milled with cnc machine.

Not pictured is a Teensy board that controls the show. I send it a request for via serial port for X energy on the caps. The Teensy charges or discharges caps to a voltage corresponding to E=1/2 * C * V^2. Pulse timing is also set via serial port. There's a weld pedal input pin, but that's also controllable via serial port.

I wouldn't mind open sourcing it once it's a bit more polished. I wonder how many people actually want to build a welder themselves with caps that have this same terminal spacing and threads.

I also made a spring loaded weld head. This part might be of more interest to the community.
e2TCHiE.png

What I think would be really useful is if you made that spring loaded head portable so you can use it with one hand and this will free the other hand to hold the nickel.
 
Back
Top